9.2 Holiday Repair and Verification
AMPP CIP Level 1 Basic Coatings Inspector
Track your progress as you read
Finished sections get a check mark.
1 Introduction and Exam Overview
AMPP CIP Level 1 Exam Overview and Certification Path
2 Chapter 2: Surface Preparation Standards
SSPC-SP Solvent and Tool Cleaning Standards Abrasive Blast Cleaning Grades Power Tool to Bare Metal, Specialty, and Water Jetting Standards
3 Surface Profile and Contaminants
Surface Profile Measurement per ASTM D4417 Visual Standards and Rust Grades Contaminant Testing and Abrasive Selection
4 Chapter 4: Coating Materials and Types
4.1 Coating Chemistry and Curing Mechanisms 4.2 Zinc-Rich Primers and Corrosion Protection 4.3 Coating Properties and Calculations 4.4 Specialty Coatings and Service Environments
5 Chapter 5 — Application Methods
5.1 Spray Application Techniques 5.2 Stripe Coating and Critical Areas
6 Chapter 6: Inspection and Defects
6.1 Application Defects and Failure Modes 6.2 Adhesion and Cure Testing 6.3 Inspector Role, Documentation, and Project Coordination
7 Ambient Conditions
Psychrometry and Instruments Dew Point Rule and Application Limits Environmental Control and Documentation
8 Chapter 8: Film Thickness Measurement
8.1 Wet Film Thickness 8.2 Dry Film Thickness Gauges and Calibration 8.3 DFT Acceptance Criteria and Procedures
9 Chapter 9: Holiday Detection
9.1 Holiday Detection Methods 9.2 Holiday Repair and Verification
10 Safety, Ethics, and Inspector Standards
OSHA Safety Standards AMPP Code of Ethics and Inspector Professional Conduct
9.2 Holiday Repair and Verification
Key Takeaways Explain This Topic AI
Mark each holiday immediately when the alarm sounds, before moving the electrode, to avoid losing the exact location.
Repair with the specified coating system and allow full cure before re-testing — testing too early can damage the repair or produce false readings from retained solvent.
Re-test each repaired area at the same voltage setting; the repair is not complete until the re-test confirms no discontinuity remains.
Pinholes are through-thickness voids often invisible to visual inspection; holiday detection finds them because the conductive sponge solution or spark bridges the gap to the substrate.
High-voltage spark testing is an ignition source — confirm the coating is solvent-free and the atmosphere is below the LEL before energizing.
Last updated: July 2026
Quick Answer: When a holiday detector signals a discontinuity, the inspector marks the location, repairs it with the specified coating system, and re-tests after the repair has cured. Holiday repair is not complete until the re-test confirms the area is discontinuity-free. Pinholes — tiny through-thickness defects that may be invisible to the naked eye — are a primary target of holiday detection. Safety hazards include fire risk from retained solvent, confined space entry during testing of tank interiors, and proper bonding and grounding of the detector to prevent stray currents.
Holiday Marking and Repair Procedure
The repair workflow follows a defined sequence that the coating inspector witnesses and documents:
Mark the holiday — Use a grease pencil, chalk, or removable marker to circle the location. Mark immediately when the alarm sounds, before moving the electrode, to avoid losing the exact spot. Do not use permanent markers or anything leaving contaminating residue.
Document the count — Record each holiday on the daily inspection report (DIR) with location, coating layer, and approximate size. Cluster patterns may indicate a systematic application problem such as spray gun distance or operator technique.
Prepare the surface — After the full survey, clean each holiday area per the project specification. Small holidays may need only solvent wiping per SSPC-SP 1; larger defects may require abrasive spot blasting or power tool cleaning to the specified preparation level.
Apply repair material — Use the specified coating system at the correct WFT and DFT. Follow the manufacturer's repair procedure — some require a different product for touch-up, a mist coat technique for pinhole fills, or stripe coating of edges first.
Allow full cure — The repair must reach the cure stage specified by the manufacturer before re-testing. Testing too early can damage the fresh repair, produce false readings from retained solvent, or create a fire hazard with high-voltage equipment.
The inspector verifies that surface preparation, WFT/DFT, and ambient conditions during repair meet the same requirements as the original application.
Re-Test After Repair
After the repair coating has cured, re-survey the repaired areas with the same detector at the same voltage setting used for the original survey. The re-test must confirm that no discontinuity remains. If a second holiday is found at the same spot, repeat the repair and retest cycle — this may indicate a recurring substrate condition (e.g., a weld undercut) requiring corrective action beyond a simple touch-up.
The inspector documents each repair and its re-test result on the non-conformance report (NCR) and DIR. Only after all holidays are repaired and verified discontinuity-free does the coating system pass the holiday detection hold point.