Study guide

Abrasive Types, Mixes, and Inspection Considerations

AMPP CIP Level 2 Certified Coatings Inspector

Track your progress as you read

Finished sections get a check mark.

1 Introduction & Exam Overview

CIP Level 2 Exam Facts and Format Prerequisites, Certification Path, and Renewal July 2026 Blueprint and Study Strategy

2 Safety

Process Safety: Equipment and Job-Site Hazards Safety Issues for Specialized Coatings and Prep Methods Environmental Safety Regulations and Regulatory Layers Containment, Waste, VOC, Silica, and Hexavalent Chromium

3 Inspection Planning

Evaluating and Applying Client Written Expectations Purpose and Cost Justification of Inspection Creating Inspection and Test Plans (ITPs) Supporting Job Specifications

4 Inspection Activities & Standards

De Facto, National, and International Standards CIP Level 2 Scope vs Level 1 Responsibilities Verifying Level 1 Work and Applying NACE/AMPP Standards

5 Corrosion Causes

Corrosion Types: General, Localized, Crevice, Flow-Assisted Corrosion Cell and Electrochemical Processes Galvanic Corrosion and Dissimilar Metals

6 Corrosion Effect & Control

Substrate Corrosion Rates, Influencing Factors, and Mitigation Cathodic Protection Systems and Effects on Coatings

7 Environmental Conditions & Inspection

Environmental Requirements and Inspection Concerns Humidity Effects on Corrosion Rates and Coating Risk Dehumidification Systems: Desiccant, Refrigerant, and Heaters Enclosures, Air Movement, and Advanced Environmental Instrumentation

8 Surface Preparation Methods

Prep Methods for Nonferrous, Wood, Concrete, and Polymeric Substrates Surface Contaminants and Acid Cleaning Pickling, Passivation, and Rinse Verification Waterjetting Methods and Removable Materials

9 Surface Prep Equipment & Standards

Concrete Surface Preparation and Standards Abrasive Types, Mixes, and Inspection Considerations Centrifugal Blast Cleaning and Portable/Remote Systems Waterjetting and Centrifugal Blast Standards AB-1/2/3 Media Standards and Special Substrates

10 Coating Application Equipment

Thermal, Electrostatic, and Polyester Spray Applications Plural-Component Systems and Specialty Coating Application Convertible vs Non-Convertible Curing and Polymerization

11 Specialty Coatings & Products

Powder Coatings and Specialized Coating Types Thick-Barrier Linings: Installation and Use Coal-Tar Enamel, Asphalt, and Tape Coatings Maintenance Coating Considerations

12 Pipeline Coatings & Hot-Dip Galvanizing

Hot-Dip Galvanizing Application Process Fusion-Bonded Epoxy (FBE) Pipeline Coating Multi-Layer Polyolefin (3LPE/3LPP) Pipeline Coatings Pipeline Field Joints and Mainline Repair Products Pipeline Coating Importance and Integrity Failure Consequences Concrete on Pipelines and Concrete Coating Standards Concrete Coating Requirements and Cure Verification

13 Coating Inspection: Assessing

Coating Surveys of Existing Systems Coating Defects, Failures, and Detection Criteria Differentiating Adhesion Testing Methods HDG Defects; Nonferrous and Concrete Coating Inspection

14 Coating Inspection: Verification

Instrument Inspections: Verification vs Calibration Concrete Coating Thickness and Destructive Tests Eddy Current and Ultrasonic DFT Methods Cathodic Disbondment and Specialized Lab Testing

15 Documentation

Level 1 Report Review and Failure Documentation for Level 3 Documenting Specialty Coatings and Developing Reports Electronic Reporting, Data Storage, and Retention Maintenance Coating Surveys and Standards Bodies Product Data Sheets and Hot-Dip Galvanizing Standards

16 Communications & Teamwork

Certified Inspector Role and CIP Level 2 Limits Owner, Contractor, and Inspector Responsibilities Pre-Job Conference and Coating Condition Assessment Surveyor Defensive Behavior and Conflict Resolution Communication

17 Ethics

Attestation and Ethics of the AMPP-Certified Inspector Addressing and Analyzing Ethical Dilemmas Positive Suggestions That Improve Job Flow and Quality

Abrasive Types, Mixes, and Inspection Considerations

Key Takeaways Explain This Topic AI

Abrasive families divide broadly into expendable mineral and slag media and recyclable metallic media, each with distinct profile and contamination behaviour.

Angularity governs profile shape: angular grit cuts an anchor pattern while round shot peens a rounded profile, and mixing them deliberately is a recognised technique.

Abrasive size and the condition of the working mix change profile more than any single operator variable on a shop line.

Abrasive cleanliness — oil, water-soluble contaminants, and fines — transfers directly to the prepared surface and defeats an otherwise correct blast.

The inspector evaluates the operating mix and the media control programme, not merely the certificate that came with the new abrasive.

Last updated: August 2026

Abrasives, Centrifugal Blast, and Portable/Remote Systems

Quick Answer: CIP Level 2 inspects abrasive type, angularity, size, cleanliness, and operating mix because media defects transfer to the steel (or other substrate) as poor profile, contamination, or embedded trash. Centrifugal blast cleaning (shop wheel machines / Wheelabrator-style) accelerates abrasive with rotating blast wheels in an enclosure with media recovery—different equipment and inspection logistics than air/pot nozzle blast, but cleanliness is still judged to the invoked SP (or equivalent) grade . Portable and remote-operated systems (vacuum blast, robotic blast, robotic UHP) extend access and dust control; the inspector still verifies cleanliness, profile, residue, and documentation .

Three Domain 5 Preparation Equipment/Materials blueprint lines sit behind this section: inspection considerations of abrasive types/mixes, centrifugal blast cleaning, and portable/remote-operated systems. These topics connect shop production lines to field specialty equipment.

Abrasives: What Level 2 Inspects

Abrasive is a process material , not just “sand in a pot.” Wrong or dirty media can fail a near-white grade even when nozzle technique looks good.

Type families (inspection awareness)

Family Examples Typical inspection notes

Mineral / slag Garnet, coal slag, copper slag, nickel slag, staurolite Common field media; check size, cleanliness, free contaminants; some slags historically scrutinized for composition/impurities

Ferrous metallic Steel grit, steel shot, chilled iron Recyclable; shot more rounded, grit more angular; watch for oil from reclaim systems

Non-ferrous specialty Aluminum oxide, glass bead, plastic, agricultural (walnut, corn cob) Used for nonferrous substrates, thin metals, or soft cleaning; embedding and substrate damage risks differ

Expendable vs recyclable One-pass mineral vs closed-loop steel Recycled systems need operating mix and cleanliness controls (see the AB media standards section later in this chapter)

Angularity

Angular particles (grit, crushed slag, angular garnet) cut the surface and develop a jagged profile preferred for many coating systems.

Rounded particles (shot, beads) tend to peen , clean, or densify with a different peak shape—often less aggressive angular cut for the same nominal size.

Mixing shot and grit is common in wheel machines to balance cleaning rate, media life, and profile. The specification/profile range decides whether the mix is acceptable—not crew preference alone.

Size (mesh / sieve)

Particle size strongly influences profile depth and cleaning rate:

Coarser media → generally deeper profile and faster scale removal (within process limits).

Finer media → shallower profile, better access into tight geometry, sometimes better finish for thin films.

Inspectors should know the specified or approved size and recognize when a load is obviously wrong (bags mislabeled, mixed lots, worn recycled fines only).

Sieve analysis awareness (field or lab) supports AB-standard verification and troubleshooting when profile drifts out of range with “the same” nozzle setup.

Cleanliness of abrasive

Contaminated abrasive re-contaminates the surface:

  • Contaminant Field effect Inspection response
  • Oil / grease Fish-eyes, adhesion loss, dark oily steel Reject media; check compressors, reclaim, storage
  • Water / moisture Clumping, reduced flow, flash issues Dry storage; reject wet bags/hoppers

Water-soluble salts Residual ionic contamination on steel Conductivity/soluble salt checks on media wash when required

Trash / organic debris Embedment, soft spots Visual inspection of media and spent dust

Dust / fines overload Poor visibility, reduced cutting efficiency, dusty surface Operating mix correction; dust collector function

Simple field screens (visual, magnet checks for metallic trash in mineral media, water-break/oil tests, supplier certificates) support hold points before large blasts.

Operating mix (working mix)

In recyclable systems, the hopper does not contain only virgin abrasive. The operating mix is the blend of particle sizes and shapes actually hitting the work after breakdown and classification:

Too many fines → low profile, dusty surface, slow cleaning.

Too much oversize / worn rounded metallic → profile and cleaning rate shift.

Failure of classifiers, scalping screens, or dust collectors shows up as mix drift.

Level 2 inspection of mixes includes: approved media type, addition rate of new abrasive, separator function, and correlation of mix condition to measured profile and cleanliness . When profile falls while pressure and technique are unchanged, check the mix before blaming the nozzle operator alone.

Inspection considerations checklist for abrasives

Approved type for substrate and coating (especially nonferrous—avoid ferrous contamination).

Size grade matches ITP/PDS/profile plan.

Angularity appropriate (grit vs shot vs blend).

Certificates and lot IDs on file when required.

Field cleanliness checks (oil, moisture, trash).

Operating mix health on recycle units.

Spent abrasive disposal and environmental rules (not inspection acceptance, but job-site reality that affects process choices).

Reading the Working Mix on a Live Job

New abrasive arrives with a certificate. The surface, however, is cleaned by whatever is circulating in the machine at that moment — the working mix (also called the operating mix). At CIP Level 2 the exam expects you to inspect the mix, not the delivery note.

Symptom on the surface Likely working-mix cause Inspector action

Profile drifting below the specified range Mix degraded to fines; too little coarse media; worn wheels or low pressure Stop releasing areas; request mix check and profile re-verification

Profile drifting above the range Coarse addition rate too high; oversized new media introduced Verify size of media being added against the procedure

Rounded rather than angular anchor pattern Grit worn to shot-like rounded particles, or shot substituted for grit Compare against the specified profile method result, not appearance alone

Surface passes visual grade but coating disbonds later Contaminated media redepositing oil or soluble salts Trigger the media verification tests before further production

Excessive dust and poor visibility Fines not being removed by the separator/classifier Report separator performance as a process defect, not a housekeeping issue

The separator is the control device

On any recycling system, the classifier/separator is what maintains the mix: it removes spent fines, dust, and debris while returning serviceable media. A separator that is out of adjustment, bypassed, or overloaded quietly changes the profile being produced across an entire shift while every individual reading still looks plausible. Level 2 practice is to treat separator condition and the media addition rate as process controls worth recording, in the same way you record gauge calibration.

What the inspector may and may not do

You verify that the contractor's media control programme exists, is being followed, and produces surfaces that meet the specified cleanliness and profile. You do not select the abrasive, set the addition rate, or redesign the recycling loop — those are means-and-methods decisions. When profile drifts out of range, the correct output is a documented non-conformance against the specified profile clause plus the supporting observation, leaving the contractor to choose the correction.