Study guide

8.7 Amine/Caustic SCC, HCl, Sour Water, and MIC (API RP 571)

API 570 Piping Inspector Exam

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: Piping Inspection Planning & Circuits

1.1 Inspection Planning, History, and Safety 1.2 Piping Circuitization and Circuit Design 1.3 Condition Monitoring Locations (CMLs) & Coverage

2 Chapter 2: Inspection Intervals & Extent of Inspection

2.1 Piping Classifications (Classes 1, 2, 3, and 4) 2.2 Thickness Inspection Intervals (Half-Life & Visual Rules) 2.3 Owner-User QA and Roles (Inspector, Engineer, Examiner)

3 Chapter 3: Calculations & Remaining Life

3.1 Corrosion Rates (Short-Term, Long-Term, and Initial Estimates) 3.2 Remaining Life and Retirement Thickness Calculations 3.3 MAWP Calculations for In-Service Piping

4 Chapter 4: ASME Codes for Piping Design

4.1 Wall Thickness Calculations for Pipe under Pressure (ASME B31.3) 4.2 Flange Ratings & P-T Limits (ASME B16.5) 4.3 Pressure & Leak Testing Rules (Hydrostatic vs. Pneumatic) 4.4 Weld Joint Quality Factors (Ej) and Casting Quality Factors (Ec) 4.5 Impact Testing, MDMT Exemption, and Charpy Requirements 4.6 Thermal Expansion Calculations (ASME B31.3 Appendix C) 4.7 Minimum Required Thickness of Permanent Blanks

5 Chapter 5: Nondestructive Examination (NDE)

5.1 Visual, Penetrant, and Magnetic Testing (VT, PT, MT) per ASME Sec V 5.2 Radiographic and Ultrasonic Testing (RT, UT) per ASME Sec V 5.3 Examiner Selection, Calibrations, and Acceptance Standards 5.4 Leak Testing per ASME Section V Article 10

6 Chapter 6: Welding Procedures & Qualifications

6.1 Reviewing WPS and PQR per ASME Section IX 6.2 Welder Performance Qualification (WPQ) and Limits 6.3 Preheating & PWHT Rules and Controls 6.4 Welding Processes, Inspection, and Metallurgy (API RP 577)

7 Chapter 7: Valves, Components, Materials & PRDs

7.1 Piping Components and Valves (API RP 574) 7.2 Positive Material Identification (PMI) (API RP 578) 7.3 Pressure Relieving Devices (PRDs) (API RP 576)

8 Chapter 8: Damage Mechanisms & Repairs

8.1 Corrosion Under Insulation (CUI) and Ambient Mechanisms 8.2 Process-Driven Damage Mechanisms (API RP 571) 8.3 Temporary and Permanent Repair Methods (ASME PCC-2 & API 570) 8.4 Soil Corrosion, Galvanic Corrosion, and Boiler Water Condensate Corrosion 8.5 Piping Rerating and Alterations (API 570) 8.6 Inspection Records, Reports, and Documentation 8.7 Amine/Caustic SCC, HCl, Sour Water, and MIC (API RP 571)

8.7 Amine/Caustic SCC, HCl, Sour Water, and MIC (API RP 571)

Key Takeaways Explain This Topic AI

Amine SCC (§3.3) produces intergranular cracking in hard, unstress-relieved carbon steel welds in alkanolamine service—hardness control and PWHT are primary mitigation.

Caustic corrosion (§3.14) is velocity- and temperature-driven metal loss; caustic SCC (§3.15) is stress-driven intergranular cracking in caustic solutions.

HCl corrosion (§3.37) causes rapid thinning and pitting on carbon steel; sour water corrosion (§3.58) attacks overhead systems with acidic aqueous H2S/NH3/CO2.

MIC (§3.45) produces under-tubercle pitting in stagnant biologically active water—not a chemical SCC mechanism.

Distinguish cracking mechanisms by material, chemistry, morphology, and location; carbon steel in amine service with hard HAZ points to amine SCC, not chloride SCC.

Last updated: July 2026

8.7 Amine/Caustic SCC, HCl, Sour Water, and MIC (API RP 571)

Six alkaline, acidic, and biological corrosion mechanisms from API RP 571 appear on the February 2026 API 570 Body of Knowledge. Inspectors must distinguish them by morphology , location , susceptible materials , inspection approach , and mitigation —not by memorizing section numbers alone. This section covers §3.3 Amine SCC , §3.14 Caustic Corrosion , §3.15 Caustic SCC , §3.37 Hydrochloric Acid Corrosion , §3.58 Sour Water Corrosion (Acidic) , and §3.45 Microbiologically Influenced Corrosion (MIC) .

Amine Stress Corrosion Cracking (API RP 571 §3.3)

Amine SCC affects carbon steel and low-alloy steels in alkanolamine sweetening systems (MEA, DEA, MDEA, etc.) when welds and heat-affected zones are high hardness or high residual stress and have not received adequate PWHT .

Morphology and Mechanism

Intergranular cracking , often initiating at weld toes , HAZ , or hard spots .

Cracks may be branching but are typically associated with alkaline amine chemistry , not chlorides.

Attack accelerated by lean amine (higher acid gas loading), elevated temperature , and CO2/H2S content.

Preferred Locations

Amine contactor/regenerator overhead and bottoms lines.

Rich/lean exchanger channel covers and inlet nozzles.

Reboiler and stripper piping.

Heat-affected zones of welds not stress-relieved.

Susceptible Materials

Carbon steel (most common); low-alloy steels without PWHT.

Hardness typically > 200 BHN in HAZ is a red flag.

Inspection and Mitigation

WFMT/MT and PT on welds; angle-beam UT for volumetric detection.

Hardness testing of welds and HAZ.

Mitigation : PWHT per B31.3 for amine service, control weld procedure to limit hardness, consider stainless upgrades only where fully evaluated for other damage modes.

Caustic Corrosion (API RP 571 §3.14)

Caustic corrosion is general or localized metal loss in sodium hydroxide (NaOH) or potassium hydroxide (KOH) solutions—not cracking driven primarily by stress.

Morphology and Mechanism

Uniform thinning , grooving , or impingement attack where velocity strips protective oxide.

Accelerated at high temperature , high concentration , and high velocity (especially > 15–20 ft/s in concentrated caustic per industry guidance).

Preferred Locations

Caustic transfer lines downstream of pumps.

Elbows and tees in concentrated caustic service.

Valve bodies and orifice locations .

Susceptible Materials

Carbon steel (forms protective magnetite at moderate conditions; breaks down at high velocity/temperature).

Copper alloys in some dilute caustic; nickel for severe service.

Inspection and Mitigation

UT thickness at high-velocity fittings.

Mitigation : velocity limits , dilution , temperature control , upgrade to nickel alloys in hot concentrated service.

Caustic Stress Corrosion Cracking (API RP 571 §3.15)

Caustic SCC (often called caustic embrittlement ) is stress-driven cracking in caustic solutions —distinct from caustic corrosion thinning.

Morphology and Mechanism

Intergranular cracking in stressed regions (welds, bends, supports).

Occurs in specific NaOH concentration/temperature windows (classically 20–50% NaOH at elevated temperature , though exam focus is concept not exact diagram memorization).

Residual weld stress or external mechanical stress required.

Preferred Locations

Steam-traced caustic lines (concentration increases from water boil-off).

Weld HAZ on caustic piping.

Cold-worked bends without stress relief.

Susceptible Materials

Carbon steel ; low-alloy steels .

Inspection and Mitigation

PT/MT on welds; review PWHT records .

Mitigation : PWHT/stress relief , avoid steam tracing without engineering controls, maintain dilute caustic where possible.

Hydrochloric Acid Corrosion (API RP 571 §3.37)

HCl corrosion is aggressive general and pitting attack from hydrochloric acid in process streams, overhead systems , or acid gas environments.

Morphology and Mechanism

Rapid uniform thinning and severe pitting .

No protective scale on carbon steel in strong HCl.

Preferred Locations

HCl injection points and downstream mixing zones.

Overhead condenser systems where HCl condenses.

Acid gas treater and regenerator overhead piping.

Susceptible Materials

Carbon steel (very low resistance).

Copper alloys in some dilute acid; nickel alloys (Hastelloy C, etc.) for severe service.

Inspection and Mitigation

UT at injection points; visual for pitting.

Mitigation : alloy upgrade , water wash/neutralization , inhibitors , lining .

Sour Water Corrosion — Acidic (API RP 571 §3.58)

Acidic sour water contains dissolved H2S , NH3 , CO2 , and often chlorides , producing low-pH aqueous condensate in refinery overhead systems.

Morphology and Mechanism

General thinning , under-deposit corrosion , pitting .

Ammonium bisulfide and acidic salts accelerate attack.

Preferred Locations

Refinery overhead systems: accumulators , reflux lines , sour water draw-offs .

Condenser outlet and separator piping.

Susceptible Materials

Carbon steel ; 300-series SS may suffer chloride SCC if chlorides present (contrast with amine SCC on CS).

Inspection and Mitigation

UT at low points; corrosion coupon/sour water sampling (pH, NH4HS, chloride).

Mitigation : pH control , neutralizer injection , corrosion inhibitors , alloy upgrades in severe circuits.

Microbiologically Influenced Corrosion (API RP 571 §3.45)

MIC results from microbial activity (sulfate-reducing bacteria, acid-producing bacteria, iron-oxidizing bacteria) creating localized chemical conditions under biofilms .

Morphology and Mechanism

Pitting under tubercles (mound-like corrosion products).

Under-deposit attack ; often very localized with adjacent unaffected metal.

Preferred Locations

Stagnant water : dead legs , hydrotest water left in lines , cooling water , buried water lines , soil with organic content .

Susceptible Materials

Carbon steel most common; stainless in some environments.

Inspection and Mitigation

Visual tubercles; UT at pits; bacterial culture and metallography for confirmation.

Mitigation : biocides , pigging , oxygen control , avoid stagnant hydrotest water , CP where applicable.

Comparison Table

Mechanism RP 571 Primary Attack Morphology Typical Location Key Susceptibility Primary NDE Mitigation

Amine SCC §3.3 Cracking IG cracks at welds/HAZ Amine contactor/regenerator piping Hard CS welds without PWHT MT/PT, UT PWHT, hardness control

Caustic corrosion §3.14 Metal loss Thinning, grooving Pump discharge, hot concentrated caustic CS at high velocity/temp UT Velocity limits, Ni alloys

Caustic SCC §3.15 Cracking IG cracks in stressed areas Steam-traced caustic, welds Stressed CS in caustic PT/MT PWHT, avoid concentration traps

HCl corrosion §3.37 Metal loss Severe thinning/pitting HCl injection, overhead acid CS in strong HCl UT, visual Alloy upgrade, neutralization

Sour water (acidic) §3.58 Metal loss General/pitting Overhead accumulators, draw-offs CS in low-pH sour water UT, sampling pH control, inhibitors

MIC §3.45 Localized pitting Pits under tubercles Stagnant water, dead legs CS in biologically active water UT, visual Biocides, flow, cleanliness

Worked Scenario: Amine SCC vs. Caustic SCC vs. Chloride SCC

An inspector examines a crack at the toe of a circumferential weld on a 2-inch carbon steel line.

Case data:

  • Factor Observation
  • Service Lean MEA amine at 180°F; no caustic in system
  • Material ASTM A106 Gr. B (carbon steel)
  • Weld history No PWHT after field repair six months ago
  • Hardness HAZ = 225 BHN
  • Crack morphology Intergranular , branching from weld toe
  • Chlorides < 50 ppm; no austenitic stainless in circuit

Eliminate chloride SCC: Cl-SCC requires austenitic stainless (300-series) at temperature with chlorides and stress. This is carbon steel —chloride SCC is not the primary mechanism (though chlorides can accelerate other attack).

Eliminate caustic SCC: No NaOH/KOH service; no steam-traced caustic concentration. Caustic SCC is unlikely.

Diagnose amine SCC: Carbon steel , hard HAZ (225 BHN) , unstress-relieved repair weld , intergranular cracking in amine service at elevated temperature —classic amine SCC (§3.3) .

Required actions: Engineer evaluates fitness-for-service; likely remove cracked weld , re-weld with qualified WPS , perform PWHT , hardness verify ≤ 200 BHN , extend MT/PT to similar welds in circuit, update inspection plan per API 570.

This distinction— material + environment + morphology + hardness —is exactly what API 570 expects when RP 571 mechanisms overlap in appearance.