Study guide
3.3 Erosion/Erosion-Corrosion & Cavitation
API 571 Corrosion and Materials Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Exam Structure, Terminology & Corrosion Fundamentals
1.1 API 571 Certification, Exam Structure & RP 571 Framework 1.2 Corrosion Science Fundamentals: Electrochemical Cells, Polarization & Passivity 1.3 Key Process Variables, Morphology Patterns & NDE Terminology
2 Chapter 2: Atmospheric, Water & Soil Corrosion
2.1 Atmospheric Corrosion & Soil Corrosion 2.2 Corrosion Under Insulation (CUI) 2.3 Cooling Water, Boiler Water & Oxygenated Process Water Corrosion
3 Chapter 3: Microbial, Electrochemical & Velocity-Induced Metal Loss
3.1 Microbiologically Influenced Corrosion (MIC) & Brine Corrosion 3.2 Galvanic Corrosion, Concentration Cell Corrosion & Dealloying 3.3 Erosion/Erosion-Corrosion & Cavitation
4 Chapter 4: Refining Sour Water & Overhead Systems Corrosion
4.1 Acidic Sour Water & Alkaline Sour Water (Ammonium Bisulfide) Corrosion 4.2 Ammonium Chloride and Amine Hydrochloride Corrosion 4.3 Flue Gas Dew Point Corrosion & Aqueous Organic Acid Corrosion
5 Chapter 5: Acid Gas, Amine & Mineral Acid Systems
5.1 Amine Corrosion & Carbon Dioxide (CO2) Sweet Corrosion 5.2 Hydrochloric Acid (HCl) Corrosion & Phenol Corrosion 5.3 Caustic Corrosion (Caustic Gouging)
6 Chapter 6: Heavy Oil, Alkylation & Specialty Acid Services
6.1 Naphthenic Acid Corrosion (NAC) 6.2 Sulfuric Acid Corrosion & Phosphoric Acid Corrosion 6.3 Hydrofluoric (HF) Acid Corrosion
7 Chapter 7: High-Temperature Oxidation & Sulfidation
7.1 High-Temperature Oxidation 7.2 Sulfidation in H2-Free Environments 7.3 High-Temperature H2/H2S Corrosion (Couper-Gorman)
8 Chapter 8: High-Temperature Carbon, Nitrogen & Ash Reactions
8.1 Carburization, Decarburization & Metal Dusting 8.2 Nitriding, Fuel Ash Corrosion & Refractory Degradation 8.3 Gaseous Oxygen-Enhanced Ignition and Combustion
9 Chapter 9: High-Temperature Hydrogen Attack & High-Temp Rupture
9.1 High-Temperature Hydrogen Attack (HTHA) Mechanisms & Nelson Curves 9.2 HTHA Inspection, Detection Methods & Mitigation 9.3 Creep, Stress Rupture & Short-Term Overheating
10 Chapter 10: Wet H2S Cracking Mechanisms
10.1 Hydrogen Blistering & Hydrogen-Induced Cracking (HIC) 10.2 Stress-Oriented Hydrogen-Induced Cracking (SOHIC) 10.3 Sulfide Stress Cracking (SSC)
11 Chapter 11: Stainless Steel & Nickel Alloy Stress Corrosion Cracking
11.1 Chloride Stress Corrosion Cracking (Cl- SCC) 11.2 Polythionic Acid Stress Corrosion Cracking (PASCC) 11.3 Caustic Stress Corrosion Cracking (Caustic Embrittlement)
12 Chapter 12: Environmental Cracking in Chemical & Refining Services
12.1 Amine Stress Corrosion Cracking 12.2 Carbonate Stress Corrosion Cracking & Ammonia SCC 12.3 HF Cracking (HSC & HF SCC of Ni Alloys) & Ethanol SCC
13 Chapter 13: Mechanical, Thermal & Corrosion Fatigue
13.1 Mechanical and Vibration-Induced Fatigue 13.2 Thermal Fatigue & Thermal Shock 13.3 Corrosion Fatigue
14 Chapter 14: Metallurgical Phase Embrittlement & Cast Iron Degradation
14.1 885 °F (475 °C) Embrittlement 14.2 Sigma Phase Embrittlement 14.3 Graphitic Corrosion of Cast Irons
15 Chapter 15: Thermal Degradation of Microstructure & Grain Structure
15.1 Graphitization 15.2 Spheroidization (Softening) 15.3 Temper Embrittlement & Strain Aging
16 Chapter 16: Toughness Loss, Welding & Dissimilar Metal Cracking
16.1 Brittle Fracture 16.2 Dissimilar Metal Weld (DMW) Cracking 16.3 Stress Relaxation Cracking (Reheat Cracking)
17 Chapter 17: Environmental Embrittlement & Specialized Hydriding
17.1 Hydrogen Embrittlement (HE) 17.2 Liquid Metal Embrittlement (LME) 17.3 Titanium Hydriding
3.3 Erosion/Erosion-Corrosion & Cavitation
Key Takeaways Explain This Topic AI
Erosion-corrosion is the synergistic acceleration of metal loss where mechanical abrasion strips protective scales (such as FeS or passive Cr2O3), exposing fresh bare metal to renewed, aggressive electrochemical attack.
Ductile alloys (carbon steel, stainless steel) experience peak erosion rates under shallow oblique impingement angles (20° to 40°), whereas brittle materials (refractories, ceramics) peak under normal 90° impingement.
Cavitation is a mechanical damage mechanism caused by vapor bubble implosion when local static pressure drops below fluid vapor pressure and recovers, generating microscopic liquid micro-jets with localized impact pressures exceeding 100,000 psi (700 MPa).
Erosion-corrosion creates directional gullies, ripples, and downstream-pointing horseshoe pits with bright, scale-free bare metal, whereas cavitation produces sharp, jagged, honeycomb-like spongy craters with no directional pattern.
Engineering mitigation of pump cavitation requires maintaining Net Positive Suction Head Available (NPSHA) safely above Net Positive Suction Head Required (NPSHR), typically with a 3 to 5 ft margin or ratio ≥1.2.
Last updated: September 2026
- Erosion and Erosion-Corrosion — API RP 571 Section 3.27
- 1. Synergistic Mechanism Description
Erosion is the purely mechanical removal of surface material resulting from the repetitive impingement of solid particles, liquid droplets, or gas bubbles suspended in a flowing fluid. Erosion-Corrosion is the synergistic acceleration of metal loss resulting from the combined, simultaneous interaction of mechanical wear and chemical or electrochemical corrosion.
In pure chemical corrosion, metal dissolution frequently slows over time because the metal forms a protective surface scale or passive film—such as iron sulfide ( F e S FeS F e S ) in sour services, iron carbonate ( F e C O 3 FeCO_3 F e C O 3 ) in sweet services, or chromium oxide ( C r 2 O 3 Cr_2O_3 C r 2 O 3 ) on stainless steels. In erosion-corrosion, turbulent fluid flow and impacting particles mechanically strip, abrade, or spall this protective film away. Bare metal is repeatedly exposed directly to the corrosive electrolyte, driving accelerated electrochemical dissolution. The resulting metal loss rate is vastly greater than the simple arithmetic sum of erosion alone plus corrosion alone. Fluid Flow + Entrained Solids / Droplets
- │
- ▼ Mechanical Shear & Impingement
- [ Protective Scale / Passive Film Removed ]
- │
- ▼ Bare Metal Substrate Exposed to Electrolyte
- [ Rapid Electrochemical Dissolution (Fe → Fe2+ + 2e-) ]
- │
- ▼ Film Re-nucleates (Repassivation attempt)
- [ Immediate Mechanical Stripping by Next Impact ]
- │
- ▼ Continuous High-Velocity Metal Loss (Grooving, Gullies, Horseshoe Pits)
- 2. Critical Factors Governing Erosion and Erosion-Corrosion
Fluid Velocity and the Power Law : Fluid velocity is the single most dominant operating variable. Metal loss rate generally increases exponentially according to an empirical power law: Wear Rate ∝ V n \text{Wear Rate} \propto V^n Wear Rate ∝ V n Where velocity exponent n n n typically ranges from 2.0 to 5.0 , depending on metallurgy, entrained particle hardness, and impingement geometry. Every material-fluid combination possesses a "critical threshold velocity" above which protective films cannot adhere.
Angle of Impingement and Material Ductility :
Ductile Materials (Carbon Steel, Austenitic Stainless Steel, Copper Alloys) : Exhibit maximum erosion rates under shallow, oblique impingement angles between 20° and 40° . At these low angles, impacting abrasive particles shear, gouge, and slice micro-chips from the metal surface.
Brittle Materials (Refractory Linings, Ceramics, Hardfacings, Cast Irons) : Exhibit maximum erosion rates under perpendicular / normal 90° impingement . Direct normal impacts induce high subsurface Hertzian stresses, causing fatigue micro-fracturing and chipping of brittle grains.
Entrained Solids Characteristics : Solid particulate concentration, size, shape, and hardness directly govern wear. Angular catalyst fines in Fluid Catalytic Cracking (FCC) units, quartz sand in crude oil gathering, and coke fines in delayed coking units represent severe erosive agents.
Multiphase Flow Regimes : Two-phase flow (such as high-velocity steam containing condensed water droplets, flashing hydrocarbons downstream of letdown valves, or gas-entrained slurries) produces violent droplet impingement and turbulent shear stresses.
3. Affected Refinery Equipment and Vulnerable Locations
Piping Geometries : Short-radius elbows, pipe tees, return bends, concentric/eccentric reducers, orifice plates, and piping downstream of flow control valves.
FCC Units : Reactor and regenerator cyclone bodies and diplegs, catalyst transfer slide valves, catalyst withdrawal lines, and slurry oil pumparound circuits.
Distillation & Hydroprocessing : Crude unit vacuum ejector systems, overhead condenser tube inlets, hydrocracker letdown valves, and delayed coker hydraulic decoking lines.
4. Morphological Hallmarks of Erosion-Corrosion
Directional Patterns : Smooth-bottomed grooves, gullies, waves, ripples, and scalloped troughs oriented strictly parallel to the direction of local fluid flow.
Horseshoe-Shaped Pits : Classic morphology consisting of crescent or horseshoe-shaped pits whose open ends point downstream (in the direction of flow).
Scale-Free Luster : Corroded surfaces exhibit a bright, clean, bare metallic luster completely free of corrosion product scales, magnetite, or iron sulfide films due to continuous mechanical polishing.
Loading diagram... Impingement Angle Mechanics & Cavitation Cycle
- Cavitation — API RP 571 Section 3.16
- 1. Physical and Thermodynamic Fundamentals
Cavitation is a purely mechanical localized degradation mechanism caused by the rapid formation, growth, and violent collapse (implosion) of vapor bubbles within a flowing liquid. Cavitation occurs without requiring solid abrasive particles or corrosive chemicals.
The thermodynamic cycle unfolds in two distinct stages:
Bubble Nucleation : When local static fluid pressure drops below the fluid's equilibrium vapor pressure ( P static < P v P_{\text{static}} < P_v P static < P v ) at the local operating temperature, the liquid instantaneously boils, creating millions of microscopic vapor cavities.
Violent Implosion : As these vapor bubbles are swept downstream into regions of recovered static pressure ( P static > P v P_{\text{static}} > P_v P static > P v ), the vapor inside condenses almost instantaneously. The surrounding liquid rushes inward to fill the void.
Because the collapse occurs adjacent to a solid metal boundary, the liquid collapses asymmetrically. The bubble deforms into a toroid, focusing a piercing, ultra-high-velocity liquid micro-jet directed straight at the metal surface. The micro-jet strikes the metal with localized impact velocities of several hundred meters per second, generating transient impact shock pressures exceeding 100,000 psi (700 MPa) .
2. Microscopic Metallurgy of Cavitation Damage
The repeated impact of localized micro-jets delivers millions of micro-water-hammer blows per second onto microscopic surface areas:
The localized impact stress exceeds the dynamic yield strength and fatigue endurance limit of the metal.
The surface undergoes severe localized plastic deformation and rapid work-hardening.
Micro-fatigue cracks initiate and propagate along crystal grain boundaries.
Metal grains fracture and tear away, leaving behind deep micro-voids and micro-spalling.
3. Vulnerable Refining Equipment
Centrifugal Pumps : Suction eye of impellers, leading tips and low-pressure suction sides of impeller vanes, casing wear rings, and pump cutwaters.
Piping Systems : Immediately downstream of pressure-reducing control valves, restrictive orifice plates, butterfly valves, and sudden pipe expansions.
Acoustic and Operational Signatures : Cavitating pumps and valves emit an unmistakable, harsh, deafening rattle and heavy vibration, universally described in refinery operations as sounding like "pumping rocks, marbles, or gravel."
4. Morphological Comparison: Erosion-Corrosion vs. Cavitation
Inspection Parameter Erosion / Erosion-Corrosion (3.27) Cavitation (3.16)
Damage Mechanism Mechanical particle/droplet impingement + electrochemical attack High-velocity micro-jet impacts from collapsing vapor cavities
Visual Appearance Smooth-bottomed grooves, gullies, ripples, and waves Deeply pitted, jagged, rough, spongy or honeycomb-like texture
Surface Directionality Strongly directional, oriented parallel to fluid flow vectors Non-directional; sharp, irregular craters with ragged edges
Pit Morphology Horseshoe-shaped pits with open ends pointing downstream Deep, closely spaced, jagged sponge craters; torn metal appearance
Surface Scale Presence Bright, shiny, polished bare metal; completely stripped of scale Dull, rough, micro-fractured bare metal; fatigue spalling
Entrained Solids Strongly dependent upon solid fines or liquid droplet volume Occurs in completely clean, solids-free homogeneous liquids
- Prevention, Mitigation & Inspection Strategies
- 1. Engineering Prevention for Erosion-Corrosion
Hydraulic Velocity Management : Sizing process piping and heat exchanger tubes to ensure operating velocities remain well below critical erosive thresholds (e.g., limiting amine solutions, sour water, and slurries to prescribed maximum velocities).
Piping Geometry Optimization : Replace short-radius elbows with long-radius bends ( R ≥ 3 D to 5 D R \ge 3D\text{ to }5D R ≥ 3 D to 5 D ) to minimize impingement angles. Install target tees (blind tees with fluid/solid buffer pockets) at changes of direction to absorb particle impacts into stagnant liquid cushions.
Metallurgy & Hardfacing Upgrades : Upgrade carbon steel to erosion-resistant alloys with rapid repassivation kinetics and superior hardness, such as 2205 Duplex Stainless Steel or nickel-base alloys. Apply cobalt-base Stellite weld overlays, tungsten carbide in nickel matrices, or thermal spray cermets to valve trim and thermowells.
Refractory Linings in FCC Units : Install hexmetal-reinforced, dense abrasion-resistant refractory linings (such as Resco AA-22S) in catalyst transfer lines, cyclone diplegs, and slide valve throats.
2. Engineering Prevention for Cavitation
Net Positive Suction Head Management : The foundational engineering defense against pump cavitation is guaranteeing that Net Positive Suction Head Available ( N P S H A NPSH_A NPS H A ) exceeds Net Positive Suction Head Required ( N P S H R NPSH_R NPS H R ) by a robust safety margin across all operating envelopes: N P S H A = P surface + H static − H friction − P vapor > N P S H R NPSH_A = P_{\text{surface}} + H_{\text{static}} - H_{\text{friction}} - P_{\text{vapor}} > NPSH_R NPS H A = P surface + H static − H friction − P vapor > NPS H R A common design practice is a margin of at least 3 to 5 ft (1.0 to 1.5 m) or an N P S H A / N P S H R NPSH_A / NPSH_R NPS H A / NPS H R ratio ≥ 1.2 to 1.3 \ge 1.2\text{ to }1.3 ≥ 1.2 to 1.3 , with pump-specific margins set by the manufacturer and project standards.
Anti-Cavitation Valve Trim : In high-pressure letdown service, install tortuous-path, multi-stage pressure reduction valve trims. These trims divide a massive pressure drop into multiple small incremental stages, ensuring local static pressure never drops below fluid vapor pressure ( P static > P v P_{\text{static}} > P_v P static > P v ).
Aeration Cushions : Injecting a small, controlled volume of non-condensable gas (air or nitrogen) into the low-pressure zone provides a compressible cushion that dampens bubble collapse shockwaves.
Cavitation-Resistant Metallurgy : Upgrade from cast iron or carbon steel to alloys with high work-hardening capabilities and superior fatigue toughness: Cobalt alloys (Stellite), Austenitic Stainless Steels (304, 316), Duplex Stainless Steels (2205), or Nickel-Aluminum Bronze (NAB).
3. Inspection & NDE Methodologies
Profile Radiography (PRT) : The premier, most reliable NDE technique for evaluating internal erosion-corrosion in small-bore piping, control valve bodies, thermowell stems, and piping elbows without removing external insulation.
Grid Ultrasonic Thickness Scanning (UT / PAUT) : Structured, high-density straight-beam and phased array ultrasonic grids mapped along the extrados (outer radius) of elbows, downstream of reducers, and around tees to quantify localized wall thinning.
Vibration & Acoustic Emission Monitoring : Online accelerometer and high-frequency acoustic emission surveillance on pump bearing housings and valve bodies to detect cavitation collapse shock frequencies in real time.
Internal Visual Examination (VT) & Liquid Penetrant Testing (PT) : Direct visual and dye penetrant inspection of pump impellers, cutwaters, and valve plugs during planned turnaround maintenance to detect micro-fatigue cracking and sponge-like cavitation craters.