Study guide
7.3 High-Temperature H2/H2S Corrosion (Couper-Gorman)
API 571 Corrosion and Materials Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Exam Structure, Terminology & Corrosion Fundamentals
1.1 API 571 Certification, Exam Structure & RP 571 Framework 1.2 Corrosion Science Fundamentals: Electrochemical Cells, Polarization & Passivity 1.3 Key Process Variables, Morphology Patterns & NDE Terminology
2 Chapter 2: Atmospheric, Water & Soil Corrosion
2.1 Atmospheric Corrosion & Soil Corrosion 2.2 Corrosion Under Insulation (CUI) 2.3 Cooling Water, Boiler Water & Oxygenated Process Water Corrosion
3 Chapter 3: Microbial, Electrochemical & Velocity-Induced Metal Loss
3.1 Microbiologically Influenced Corrosion (MIC) & Brine Corrosion 3.2 Galvanic Corrosion, Concentration Cell Corrosion & Dealloying 3.3 Erosion/Erosion-Corrosion & Cavitation
4 Chapter 4: Refining Sour Water & Overhead Systems Corrosion
4.1 Acidic Sour Water & Alkaline Sour Water (Ammonium Bisulfide) Corrosion 4.2 Ammonium Chloride and Amine Hydrochloride Corrosion 4.3 Flue Gas Dew Point Corrosion & Aqueous Organic Acid Corrosion
5 Chapter 5: Acid Gas, Amine & Mineral Acid Systems
5.1 Amine Corrosion & Carbon Dioxide (CO2) Sweet Corrosion 5.2 Hydrochloric Acid (HCl) Corrosion & Phenol Corrosion 5.3 Caustic Corrosion (Caustic Gouging)
6 Chapter 6: Heavy Oil, Alkylation & Specialty Acid Services
6.1 Naphthenic Acid Corrosion (NAC) 6.2 Sulfuric Acid Corrosion & Phosphoric Acid Corrosion 6.3 Hydrofluoric (HF) Acid Corrosion
7 Chapter 7: High-Temperature Oxidation & Sulfidation
7.1 High-Temperature Oxidation 7.2 Sulfidation in H2-Free Environments 7.3 High-Temperature H2/H2S Corrosion (Couper-Gorman)
8 Chapter 8: High-Temperature Carbon, Nitrogen & Ash Reactions
8.1 Carburization, Decarburization & Metal Dusting 8.2 Nitriding, Fuel Ash Corrosion & Refractory Degradation 8.3 Gaseous Oxygen-Enhanced Ignition and Combustion
9 Chapter 9: High-Temperature Hydrogen Attack & High-Temp Rupture
9.1 High-Temperature Hydrogen Attack (HTHA) Mechanisms & Nelson Curves 9.2 HTHA Inspection, Detection Methods & Mitigation 9.3 Creep, Stress Rupture & Short-Term Overheating
10 Chapter 10: Wet H2S Cracking Mechanisms
10.1 Hydrogen Blistering & Hydrogen-Induced Cracking (HIC) 10.2 Stress-Oriented Hydrogen-Induced Cracking (SOHIC) 10.3 Sulfide Stress Cracking (SSC)
11 Chapter 11: Stainless Steel & Nickel Alloy Stress Corrosion Cracking
11.1 Chloride Stress Corrosion Cracking (Cl- SCC) 11.2 Polythionic Acid Stress Corrosion Cracking (PASCC) 11.3 Caustic Stress Corrosion Cracking (Caustic Embrittlement)
12 Chapter 12: Environmental Cracking in Chemical & Refining Services
12.1 Amine Stress Corrosion Cracking 12.2 Carbonate Stress Corrosion Cracking & Ammonia SCC 12.3 HF Cracking (HSC & HF SCC of Ni Alloys) & Ethanol SCC
13 Chapter 13: Mechanical, Thermal & Corrosion Fatigue
13.1 Mechanical and Vibration-Induced Fatigue 13.2 Thermal Fatigue & Thermal Shock 13.3 Corrosion Fatigue
14 Chapter 14: Metallurgical Phase Embrittlement & Cast Iron Degradation
14.1 885 °F (475 °C) Embrittlement 14.2 Sigma Phase Embrittlement 14.3 Graphitic Corrosion of Cast Irons
15 Chapter 15: Thermal Degradation of Microstructure & Grain Structure
15.1 Graphitization 15.2 Spheroidization (Softening) 15.3 Temper Embrittlement & Strain Aging
16 Chapter 16: Toughness Loss, Welding & Dissimilar Metal Cracking
16.1 Brittle Fracture 16.2 Dissimilar Metal Weld (DMW) Cracking 16.3 Stress Relaxation Cracking (Reheat Cracking)
17 Chapter 17: Environmental Embrittlement & Specialized Hydriding
17.1 Hydrogen Embrittlement (HE) 17.2 Liquid Metal Embrittlement (LME) 17.3 Titanium Hydriding
7.3 High-Temperature H2/H2S Corrosion (Couper-Gorman)
Key Takeaways Explain This Topic AI
High-temperature H2/H2S corrosion operates in hydroprocessing units (hydrotreaters, hydrocrackers, catalytic reformer pretreaters) where hydrogen gas and hydrogen sulfide coexist at temperatures above 450 °F (232 °C).
Hydrogen gas exacerbates sulfidation by catalytically reducing organosulfur molecules (including stable thiophenes) into reactive H2S, preventing the formation of protective coke or oxide films, and generating a highly defective, non-protective iron sulfide scale.
API RP 571 ranks resistance as carbon steel < low alloy steels < 400 series SS < 300 series SS; there is little improvement until about 7% to 9% Cr, and at least 9Cr-1Mo is normally needed for a practical improvement over carbon steel.
Modified Couper-Gorman curves estimate rates from temperature and H2S concentration; because of higher H2S partial pressure, gas oil hydrotreaters and hydrocrackers generally corrode faster than lower-pressure naphtha hydrotreaters.
To prevent Polythionic Acid Stress Corrosion Cracking (PASCC) during turnaround outages, 300-series stainless steel components must be stabilized grades (Type 321 or Type 347) or low-carbon grades thermally stabilized, and protected via alkaline wash or nitrogen purges per NACE SP0170.
Last updated: September 2026
7.3 High-Temperature H2/H2S Corrosion (Couper-Gorman)
High-Temperature H 2 / H 2 S \text{H}_2/\text{H}_2\text{S} H 2 / H 2 S Corrosion is an aggressive form of sulfidation that occurs in petroleum refining hydroprocessing units where hydrogen gas ( H 2 \text{H}_2 H 2 ) and hydrogen sulfide ( H 2 S \text{H}_2\text{S} H 2 S ) are simultaneously present at elevated temperatures and pressures. Documented under API RP 571 Section 3.35 , this mechanism governs materials selection and equipment integrity across hydrodesulfurization (HDS) units, distillate hydrotreaters (DHT), gas oil hydrotreaters, hydrocrackers, and catalytic reformer pretreaters.
While high-temperature sulfidation in H 2 \text{H}_2 H 2 -free environments is governed by the modified McConomy curves, the presence of molecular hydrogen fundamentally alters both the reaction thermodynamics and the physical nature of the resulting scale. High-temperature H 2 / H 2 S \text{H}_2/\text{H}_2\text{S} H 2 / H 2 S corrosion initiates at a lower temperature threshold of 450 °F (232 °C) and produces significantly higher metal loss rates than H 2 \text{H}_2 H 2 -free sulfidation at identical temperatures and sulfur concentrations. [ Hydroprocessing Stream: High-Pressure H2 + H2S ]
- Operating Temp > 450 °F (232 °C)
- |
- v
- +-----------------------------------------------------------------+
- | Porous, Friable, Non-Adherent FeS Scale |
- | H2 Prevents Passive Oxide & Coke Film Formation |
- | Rapid Outward Fe2+ Diffusion & Rapid Scale Spalling |
- +-----------------------------------------------------------------+
- ^
- | Rapid Metal Dissolution
- +-----------------------------------------------------------------+
- | Substrate: Carbon Steel & Cr-Mo Steels (1.25Cr to 9Cr) |
- | ** Little Benefit from Cr until about 7-9% Cr ** |
- | 12Cr better; 300 Series SS (321, 347) Highly Resistant |
- +-----------------------------------------------------------------+
- Chemical Reaction Kinetics and The Transforming Influence of Hydrogen
The fundamental chemical reaction governing H 2 / H 2 S \text{H}_2/\text{H}_2\text{S} H 2 / H 2 S corrosion is the reversible reaction between iron and hydrogen sulfide: Fe + H 2 S ⟷ FeS + H 2 \text{Fe} + \text{H}_2\text{S} \longleftrightarrow \text{FeS} + \text{H}_2 Fe + H 2 S ⟷ FeS + H 2
Although the stoichiometric reaction indicates that molecular hydrogen is a product of the corrosion reaction, the presence of high-pressure hydrogen gas in the bulk process environment drives three catastrophic kinetic and metallurgical transformations:
Reduction of Organosulfur into Reactive H2S: In H 2 \text{H}_2 H 2 -free service, stable thiophenic ring sulfur compounds pass through equipment without reacting. In hydroprocessing units, high-pressure hydrogen catalytically hydrogenates and hydrocracks even the most refractory thiophenes and dibenzothiophenes into gaseous, highly reactive H 2 S \text{H}_2\text{S} H 2 S . Thus, virtually 100% of the sulfur in the process stream is converted into active corrodent .
Suppression of Protective Coke and Oxide Barriers: In H 2 \text{H}_2 H 2 -free service, semi-protective coke films and trace oxide scales help moderate sulfidation kinetics. High-pressure hydrogen creates an intensely reducing chemical atmosphere that completely eliminates oxide films and retards coke accumulation on metal surfaces, leaving the base metal continuously exposed.
Formation of Highly Defective, Fragile FeS Scale: The iron sulfide scale formed in the presence of H 2 \text{H}_2 H 2 is structurally disorganized, highly porous, and populated by extreme cation vacancy densities. The scale exhibits virtually zero adherence to the steel substrate, flaking and spalling continuously during operation and leaving bare steel in direct contact with H 2 S \text{H}_2\text{S} H 2 S .
The Couper-Gorman Curves and Key Operating Variables
Corrosion rates in high-temperature H 2 / H 2 S \text{H}_2/\text{H}_2\text{S} H 2 / H 2 S service are predicted using the Couper-Gorman Curves , published by A.S. Couper and J.W. Gorman in 1971 based on extensive NACE Committee T-8 surveys and verified refinery operating data, and reproduced as modified curves in API RP 571 Section 3.35 and API RP 939-C.
Primary Process Variables Governing Corrosion Rates
Temperature: Corrosion initiates at 450 °F (232 °C) . Corrosion rates increase exponentially with temperature up to approximately 750 °F to 800 °F (399 °C to 427 °C) . Above 800 °F (427 °C), the rate of increase often plateaus or may even decrease slightly due to thermodynamic equilibrium shifts in the reversible reaction Fe + H 2 S ⟷ FeS + H 2 \text{Fe} + \text{H}_2\text{S} \longleftrightarrow \text{FeS} + \text{H}_2 Fe + H 2 S ⟷ FeS + H 2 and changes in sulfide scale morphology.
H2S Concentration (Partial Pressure / Mol%): Evaluated across the spectrum from 0.01 mol% to 10.0 mol% H 2 S \text{H}_2\text{S} H 2 S in the process vapor phase. Corrosion rate increases with the partial pressure of H 2 S \text{H}_2\text{S} H 2 S ( P H 2 S = y H 2 S ⋅ P total P_{\text{H}_2\text{S}} = y_{\text{H}_2\text{S}} \cdot P_{\text{total}} P H 2 S = y H 2 S ⋅ P total ).
Unit Pressure and Stream Type (Naphtha vs. Gas Oil): The modified Couper-Gorman curves include separate correlations for naphtha and gas oil desulfurizers. API RP 571 notes that, primarily because of higher H2S partial pressure, corrosion rates in higher-pressure units such as gas oil hydrotreaters (desulfurizers) and hydrocrackers are generally higher than in lower-pressure naphtha hydrotreaters.
Vapor/Liquid Ratio: RP 571 lists the vapor-liquid ratio among the critical factors, together with temperature, the presence of hydrogen, H2S concentration (partial pressure), and alloy composition. Corrosion Rate (mpy) - Naphtha Service at 1.0 mol% H2S
- 100 | Carbon Steel (low-Cr steels only slightly lower)
- 80 | * * *
- 60 | * * *
- 40 | * * *
- 20 | * * *
- 0 +--------------* * *-----------------------[ 300 Series Austenitic SS < 2 mpy ]
- 450°F 550°F 650°F 750°F 850°F
- Temperature (°F)
Chromium Content: Why Low Alloy Steels Help Only a Little
A heavily tested contrast in RP 571 is how differently chromium performs in H2-free sulfidation (Section 3.61) and in H2/H2S service (Section 3.35).
Comparison: Modified McConomy vs. Modified Couper-Gorman
Process Environment Behavior of Low Alloy Cr-Mo Steels Governing Idea
H2-Free Sulfidation (modified McConomy curves) Resistance improves progressively as chromium increases (5Cr and 9Cr are common upgrades) Chromium enters the sulfide scale and slows iron diffusion
High-Temp H2/H2S (modified Couper-Gorman curves) Little improvement until about 7% to 9% Cr ; at least 9Cr-1Mo is normally needed for a practical improvement over carbon steel Hydrogen keeps the scale iron-rich and non-protective at low chromium levels
Order of Increasing Resistance (RP 571)
Carbon steel → low alloy steels → 400 series SS → 300 series SS. Chromium-containing nickel alloys behave like stainless steels with similar chromium levels.
9Cr-1Mo: the lowest alloy that normally gives a useful improvement over carbon steel.
12Cr Steels (Type 405 / 410): Better resistance than 9Cr, but prone to 885 °F (475 °C) embrittlement and limited weldability, so they are used mainly as cladding or internals.
300-Series Austenitic Stainless Steels (Type 304L, 316L, 321, 347): Provide outstanding corrosion resistance. With 18% to 20% Cr and 8% to 12% Ni, these alloys form a dense, adherent, microscopic chromium-rich sulfide/spinel barrier layer ( Cr 2 S 3 \text{Cr}_2\text{S}_3 Cr 2 S 3 / FeCr 2 S 4 \text{FeCr}_2\text{S}_4 FeCr 2 S 4 ). Corrosion rates are typically 10 to 50 times lower than carbon steel, consistently remaining below 1 to 2 mpy under standard hydroprocessing conditions.
Nickel-Base Alloys (Alloy 825, Alloy 625): Alloy 825 (UNS N08825, ~42% Ni, 22% Cr, 3% Mo) and Alloy 625 (UNS N06625) provide near-total immunity. Note: High-nickel alloys containing >60% Ni with low chromium (such as Alloy 200 or Monel 400) must never be used in high-temperature H 2 S \text{H}_2\text{S} H 2 S environments due to the formation of a low-melting nickel sulfide eutectic ( Ni 3 S 2 \text{Ni}_3\text{S}_2 Ni 3 S 2 / Ni) that melts catastrophically at 1175 °F (635 °C) .
Loading diagram... High-Temp H2/H2S Corrosion: Reaction Kinetics, Material Thresholds, and PASCC Risk
Reactor Construction, Cladding Strategies, and Polythionic Acid SCC
Because hydroprocessing reactors, exchangers, and separator vessels operate under severe combinations of high pressure (500 to 3000 psig), high temperature (500 °F to 850 °F), and high hydrogen partial pressure, equipment cannot be fabricated from solid austenitic stainless steel due to cost, thermal fatigue stress, and ASME section thickness limitations.
1. Dual-Metallurgy Construction Strategy
Refineries utilize a dual-metallurgy engineering design:
Pressure Boundary Base Metal: Heavy-wall shell plates and forgings are fabricated from low-alloy steels—specifically 2.25Cr-1Mo or 2.25Cr-1Mo-0.25V (ASTM A387 Gr 22 / Gr 22V, ASTM A336 Gr F22 / F22V). These alloys provide high mechanical tensile strength, superior creep resistance, and verified resistance to High-Temperature Hydrogen Attack (HTHA) per the API RP 941 Nelson curves.
Corrosion Barrier Cladding: The internal process-wetted surfaces are protected with a 3 mm to 5 mm (1/8 in.) internal layer of austenitic stainless steel , applied via roll-bonded clad plate or multi-pass automated submerged arc / electroslag weld overlay (typically an initial Type 309L buffer layer followed by a Type 347 finish layer).
2. The Threat of Sensitization and Polythionic Acid SCC (PASCC)
While 300-series stainless steels solve Couper-Gorman corrosion, they introduce an acute shutdown failure mechanism: Polythionic Acid Stress Corrosion Cracking (PASCC) , documented in API RP 571 Section 3.52 .
Sensitization Mechanism: When standard austenitic stainless steels (such as Type 304 or Type 316) are heated within the sensitization range of 750 °F to 1500 °F (399 °C to 816 °C) —which occurs during reactor post-weld heat treatment (PWHT at ~1250 °F) or during high-temperature operation—carbon atoms diffuse rapidly to austenite grain boundaries, precipitating chromium carbides: 23 Cr + 6 C ⟶ Cr 23 C 6 23\text{Cr} + 6\text{C} \longrightarrow \text{Cr}_{23}\text{C}_6 23 Cr + 6 C ⟶ Cr 23 C 6 This precipitates chromium from the adjacent metallic matrix, depleting localized grain boundary chromium content to well below the 12% passivity limit.
Shutdown PASCC Attack: During turnaround shutdowns, ambient oxygen and liquid water enter the opened vessel, reacting with internal iron sulfide scale to form polythionic acids ( H 2 S x O 6 \text{H}_2\text{S}_x\text{O}_6 H 2 S x O 6 ) : FeS + O 2 + H 2 O ⟶ H 2 S x O 6 \text{FeS} + \text{O}_2 + \text{H}_2\text{O} \longrightarrow \text{H}_2\text{S}_x\text{O}_6 FeS + O 2 + H 2 O ⟶ H 2 S x O 6 In the presence of residual weld or fabrication stresses, polythionic acid attacks the sensitized, chromium-depleted grain boundaries, causing rapid, catastrophic intergranular cracking that can propagate through an entire vessel wall or piping spool within hours.
3. Prevention Guidelines (NACE SP0170)
To eliminate PASCC risk in hydroprocessing units:
Specify Stabilized Stainless Steel Grades: Specify Type 347 (stabilized with niobium/columbium: Nb ≥ 10 × C \text{Nb} \ge 10 \times \text{C} Nb ≥ 10 × C ) or Type 321 (stabilized with titanium: Ti ≥ 5 × C \text{Ti} \ge 5 \times \text{C} Ti ≥ 5 × C ). Niobium and titanium form stable carbo-nitrides at elevated temperatures, tying up carbon and preventing chromium carbide precipitation.
Specify Thermal Stabilization Heat Treatment: Type 321 and 347 base materials and weldments are thermally stabilized by heating to 1600 °F to 1650 °F (871 °C to 899 °C) for 4 hours , ensuring complete carbon precipitation as TiC or NbC.
Implement NACE SP0170 Shutdown Procedures: Prior to opening hydroprocessing equipment to air, internal surfaces must be neutralized with an alkaline wash solution (typically 1.0 to 2.0 wt% sodium carbonate / soda ash ), or purged continuously with dry nitrogen maintaining a dew point below -40 °F (-40 °C) to prevent liquid moisture condensation.
- Affected Process Units, Damage Morphology, and Inspection Strategies
- 1. High-Risk Refinery Units and Circuits
Hydrodesulfurization (HDS) & Hydrotreating Units (NHT, DHT, VGO HT): Feed furnace radiant tubes, reactor transfer lines, reactor inlet diffusers, catalyst support grids, reactor effluent piping, and effluent heat exchangers upstream of the reactor effluent air cooler (REAC) water wash injection point.
Hydrocracking Units: 1st and 2nd stage hydrocracker charge heaters, interstage reactor piping, reactor effluent exchangers, and hot high-pressure separator (HHPS) vessels.
Catalytic Reforming Units: Naphtha pretreater charge heaters, reactors, and recycle gas piping containing H 2 \text{H}_2 H 2 and H 2 S \text{H}_2\text{S} H 2 S .
Downstream of Hydrogen Injection: RP 571 notes noticeable increases in corrosion rate downstream of the hydrogen injection point, where the mechanism changes from H2-free sulfidation to H2/H2S corrosion.
2. Macroscopic Appearance and Scale Fouling Hazards
Appearance: Uniform loss of thickness from the process side under an iron sulfide scale. RP 571 notes that the scale is about five times the volume of the metal lost and may be multilayered, and that a tightly adherent, shiny gray scale can be mistaken for unaffected metal .
Downstream Catalyst Bed Fouling ("Scale Blinding"): In fired heaters fabricated from under-alloyed carbon steel or Cr-Mo steel, heavy iron sulfide scale continuously exfoliates into the process fluid. This scale debris is carried directly into downstream hydroprocessing reactors, settling across the top of the catalyst bed. Known as scale blinding , this debris chokes flow channels, generating severe reactor bed differential pressure ( Δ P \Delta P Δ P ) spikes that force premature unit shutdowns.
3. Non-Destructive Examination (NDE) and Materials Verification
100% Positive Material Identification (PMI): Because carbon steel and low-chromium steels have far less resistance than the specified stainless steel, accidental installation of a low-alloy spool piece in an austenitic stainless steel circuit results in catastrophic rapid failure. Specifications mandate 100% PMI testing (via XRF or spark-OES) on all field welds, shop fabrications, flanges, fittings, and thermowells.
Profile Radiography (PRT): Deployed on piping circuits, thermowells, and small-bore fittings to verify remaining wall thickness and detect internal scale shedding without insulation removal.
Automated Ultrasonic Thickness Scanning (AUT): High-density ultrasonic grid mapping on furnace tubes, transfer line elbows, and separator shells to establish true corrosion rates.
Internal Dye Penetrant Inspection (PT): Applied to stainless steel cladding, weld overlays, and internal attachment welds during turnarounds to detect intergranular polythionic acid stress corrosion cracking.