Study guide
1.2 The Hysteresis Loop and B-H Curve
ASNT NDT Level III Magnetic Particle Testing MT
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Magnetization Principles and Physics
1.1 Magnetic Fields, Poles, and Domain Theory 1.2 The Hysteresis Loop and B-H Curve 1.3 Longitudinal vs. Circular Magnetization Fields 1.4 Magnetic Flux Leakage Theory and Defect Detectability 1.5 Probability of Detection, Reliability, and Technique Validation
2 Chapter 2: Direct Contact and Longitudinal Magnetization Techniques
2.1 Head Shots and Direct Contact Techniques 2.2 Prod Techniques and Localized Circular Magnetization 2.3 Longitudinal Coil Magnetization and Calculations
3 Chapter 3: Central Conductor, Yoke, and Vector Magnetization
3.1 Central Conductor (Induced Current) Techniques 3.2 Electromagnetic Yokes and Portable Field Techniques 3.3 Multidirectional and Vector Magnetization
4 Chapter 4: Magnetic Particles and Carrier Vehicles
4.1 Particle Characteristics: Physical, Magnetic, and Optical Properties 4.2 Dry Powder Systems and Application Techniques 4.3 Wet Particle Systems: Water vs. Petroleum Distillate Vehicles 4.4 Bath Concentration, Centrifuge Settling, and Maintenance
5 Chapter 5: Electrical Waveforms, Equipment, and Demagnetization
5.1 Current Waveforms and Penetration: AC, HWDC, FWDC, and 3-Phase FWDC 5.2 Stationary Wet Horizontal Benches and Portable Units 5.3 Demagnetization Principles, Methods, and Residual Field Limits
6 Chapter 6: Quality Control, Calibration, and System Performance
6.1 Lighting and Viewing Environment Requirements 6.2 Field Indicators and System Performance Check Devices 6.3 Equipment Calibration and Periodic Verifications 6.4 Bath Contamination, Water Break, and Cleanliness Tests
7 Chapter 7: Inherent and Primary Processing Discontinuities
7.1 Ingot and Casting Discontinuities 7.2 Wrought and Primary Forming Discontinuities 7.3 Secondary Processing Discontinuities: Machining and Heat Treating
8 Chapter 8: Service Discontinuities and Indication Evaluation
8.1 Service Discontinuities: Fatigue, Stress Corrosion, and Creep 8.2 Welding Discontinuities and Weldment Examination 8.3 Indication Classification: Relevant, Non-Relevant, and False 8.4 MT Reports, Records, and Documentation Review
9 Chapter 9: Industry Codes, Standards, and Acceptance Criteria
9.1 ASME Section V, Article 7 (Mandatory MT Requirements) 9.2 ASTM E1444 vs. ASTM E709 vs. ISO 9934 9.3 Acceptance Criteria in Fabrication Codes: ASME VIII, AWS D1.1, and API 1104 9.4 Reviewing Client Requirements and Product-Form MT Specifications
10 Chapter 10: Level III Responsibilities, Procedures, Training, and Program Oversight
10.1 Level III Duties, SNT-TC-1A, and ANSI/ASNT CP-189 10.2 Preparation and Qualification of MT Written Procedures 10.3 Safety, Environmental, and Health Considerations in MT 10.4 Developing and Delivering MT Training Programs 10.5 Developing and Administering MT Qualification Examinations 10.6 MT Program Audits, Supplier Oversight, and Personnel Performance
1.2 The Hysteresis Loop and B-H Curve
Key Takeaways Explain This Topic AI
The B-H hysteresis loop plots magnetic flux density (B) against magnetizing force (H), demonstrating that magnetic induction lags behind changes in the external magnetizing effort.
Key quantitative loop parameters include magnetic saturation (B_sat), residual induction or retentivity (B_r) remaining at H = 0, and coercive force (H_c) required to depress induction back to zero.
The enclosed geometric area of the hysteresis loop is directly proportional to the energy dissipated as heat per cycle, distinguishing narrow-loop soft materials from broad-loop hard alloys.
The continuous magnetization method is mandatory for magnetically soft alloys due to their low retentivity, whereas the residual method is strictly restricted to high-retentivity, high-coercivity hard materials.
Last updated: September 2026
- 1.2 The Hysteresis Loop and B-H Curve
- Anatomy of the B-H Curve and Hysteresis Loop
The magnetic hysteresis loop (or B-H curve) is the primary graphical fingerprint of a material's magnetic performance under an applied magnetizing force. It characterizes the non-linear relationship between the external magnetic field intensity ( H H H ) and the resulting internal magnetic induction ( B B B ).
Coordinate Axes and Units
Horizontal Axis ( H H H - Magnetizing Force): Also referred to as magnetic field strength or field intensity, H H H represents the external magnetizing effort applied to the material.
In the CGS electromagnetic system, H H H is measured in Oersteds (Oe) , where 1 Oe = 1 Gilbert per centimeter = 1000 4 π A/m ≈ 79.577 A/m 1\text{ Oe} = 1\text{ Gilbert per centimeter} = \frac{1000}{4\pi}\text{ A/m} \approx 79.577\text{ A/m} 1 Oe = 1 Gilbert per centimeter = 4 π 1000 A/m ≈ 79.577 A/m .
In the SI system, H H H is measured in Amperes per meter (A/m) .
Vertical Axis ( B B B - Magnetic Flux Density): Also known as magnetic induction, B B B quantifies the total concentration of magnetic lines of force per unit cross-sectional area established inside the material.
In the CGS electromagnetic system, B B B is measured in Gauss (G) , where 1 Gauss = 1 Maxwell per square centimeter 1\text{ Gauss} = 1\text{ Maxwell per square centimeter} 1 Gauss = 1 Maxwell per square centimeter ( 1 line/cm 2 1\text{ line/cm}^2 1 line/cm 2 ).
In the SI system, B B B is measured in Tesla (T) , where 1 Tesla = 1 Weber per square meter 1\text{ Tesla} = 1\text{ Weber per square meter} 1 Tesla = 1 Weber per square meter ( 1 Wb/m 2 1\text{ Wb/m}^2 1 Wb/m 2 ).
Conversion: 1 Tesla = 10 , 000 Gauss 1\text{ Tesla} = 10,000\text{ Gauss} 1 Tesla = 10 , 000 Gauss ( 1 mT = 10 Gauss 1\text{ mT} = 10\text{ Gauss} 1 mT = 10 Gauss ).
The Virgin (Initial) Magnetization Curve
When a completely demagnetized ferromagnetic specimen ( B = 0 , H = 0 B=0, H=0 B = 0 , H = 0 ) is subjected to an incrementally increasing magnetizing force, the resulting flux density traces a unique non-linear path called the virgin or initial magnetization curve:
Initial Region (Low H H H ): The curve starts at the origin ( 0 , 0 ) (0,0) ( 0 , 0 ) with a modest slope. Magnetization proceeds via reversible domain wall displacement. The slope at the origin defines initial permeability ( μ i = lim H → 0 B H \mu_i = \lim_{H \to 0} \frac{B}{H} μ i = lim H → 0 H B ).
Knee Region (Moderate H H H ): The curve steepens dramatically as irreversible domain wall movement and Barkhausen jumps occur. Here, the material exhibits its maximum permeability ( μ m a x \mu_{max} μ ma x ), where a small increase in H H H yields a massive surge in flux density B B B .
Saturation Plateau (High H H H ): The curve bends horizontally as domain rotation completes. The slope flattens out to μ 0 \mu_0 μ 0 . The material reaches magnetic saturation ( B s a t B_{sat} B s a t ).
The Phenomenon of Hysteresis
The term hysteresis is derived from the ancient Greek word υ ˙ σ τ ϵ ˊ ρ η σ ι ς \dot{\upsilon}\sigma\tau\acute{\epsilon}\rho\eta\sigma\iota\varsigma υ ˙ σ τ ϵ ˊ ρ η σ ι ς , meaning "to lag behind." In magnetic physics, it describes the empirical fact that the magnetic flux density ( B B B ) lags behind the applied magnetizing force ( H H H ). Because domain wall movements encounter physical pinning and require finite energy to overcome microstructural obstacles, the reduction of H H H back to zero does not return B B B to zero. The magnetization curve follows an entirely different descending trajectory, forming a closed loop upon cyclic reversal.
- Key Parameters: B s a t B_{sat} B s a t , B r B_r B r , H c H_c H c , and Loop Energy Loss
- 1. Magnetic Saturation ( B s a t B_{sat} B s a t )
Magnetic saturation represents the maximum achievable magnetic flux density induced within the material under practical magnetizing fields. At + B s a t +B_{sat} + B s a t , all magnetic domain vectors are oriented parallel to the external field vector. Further increases in H H H yield no additional domain contribution; the curve increases strictly at the rate of Δ B = μ 0 Δ H \Delta B = \mu_0 \Delta H Δ B = μ 0 Δ H . In structural carbon steels, saturation flux density typically occurs between 14 , 000 14,000 14 , 000 and 21 , 500 Gauss 21,500\text{ Gauss} 21 , 500 Gauss ( 1.4 1.4 1.4 to 2.15 Tesla 2.15\text{ Tesla} 2.15 Tesla ).
2. Residual Induction ( B r B_r B r ) and Retentivity
When the magnetizing force H H H is progressively reduced from the saturation point back to zero ( H = 0 H = 0 H = 0 ), the flux density does not collapse to zero. A substantial portion of magnetic flux remains locked inside the material:
Residual Induction ( B r B_r B r or Remanence): The actual magnetic flux density remaining in a specific magnetic circuit after the magnetizing force is reduced to zero.
Retentivity: The maximum value of residual induction that a material can retain when magnetized to full saturation. Retentivity is an inherent material property, whereas remanence depends upon the peak magnetizing force achieved prior to field removal.
3. Coercive Force ( H c H_c H c ) and Coercivity
To eliminate the residual induction and drive the internal flux density B B B back to zero, a reverse magnetizing force must be applied:
Coercive Force ( H c H_c H c ): The reverse magnetizing force (measured in Oersteds or A/m) required to reduce the residual flux density to zero.
Coercivity: The specific value of coercive force required to reduce the flux density to zero after the material has been magnetized to full saturation. Materials with high coercivity fiercely resist demagnetization and external magnetic shock.
4. Area of the Hysteresis Loop and Energy Dissipation
The enclosed geometric area of the B-H loop possesses direct physical significance: it represents the volumetric energy lost per magnetization cycle: W h = ∮ H d B W_h = \oint H \, dB W h = ∮ H d B
This energy loss is converted irreversibly into thermal energy (heat) as domain walls snap past microstructural pinning obstacles. In alternating current (AC) magnetic particle equipment, materials with broad hysteresis loops will heat up rapidly during continuous testing cycles due to substantial hysteresis losses.
Magnetically Soft vs. Magnetically Hard Materials
In NDT engineering and metallurgical classification, ferromagnetic materials are categorized as either magnetically "soft" or magnetically "hard." This distinction depends not on mechanical hardness alone, but on domain mobility and loop morphology.
Magnetically Soft Materials
Magnetically soft materials permit rapid, easy domain wall motion with minimal energetic resistance.
Loop Characteristics: Narrow, tall, slender hysteresis loop; steep slope (very high permeability μ \mu μ ); low coercive force ( H c < 10 Oe H_c < 10\text{ Oe} H c < 10 Oe , often < 1 Oe < 1\text{ Oe} < 1 Oe ); low retentivity; small enclosed loop area (minimal hysteresis heat loss).
Representative Alloys: Low-carbon mild steels (AISI 1008, 1018, ASTM A36), commercially pure iron (Armco iron), soft silicon steels (electrical transformer sheet), annealed ductile irons.
NDT Behavior: Readily magnetized to saturation with modest electrical amperage; loses magnetic flux rapidly upon current cessation; extremely easy to demagnetize with standard AC coil equipment.
Magnetically Hard Materials
Magnetically hard materials contain dense microstructural barriers—such as martensitic needle plates, fine carbide dispersions, high residual lattice stresses, or heavy dislocation forests—that aggressively pin domain walls.
Loop Characteristics: Wide, broad, squat hysteresis loop; gradual slope (low permeability μ \mu μ ); high coercive force ( H c > 50 to 100 Oe H_c > 50\text{ to }100\text{ Oe} H c > 50 to 100 Oe , exceeding 1 , 000 Oe 1,000\text{ Oe} 1 , 000 Oe in permanent magnets); high retentivity; large enclosed loop area (substantial hysteresis heat loss).
Representative Alloys: High-carbon tool steels (D2, M2, O1), quenched and tempered alloy steels (AISI 4140, 4340, 300M in high-hardness conditions), martensitic stainless steels (AISI 440C), precipitation-hardened steels (17-4 PH H900), permanent magnet alloys (Alnico, Samarium-Cobalt, Neodymium-Iron-Boron).
NDT Behavior: Requires high magnetizing amperages to reach saturation; retains strong, stable residual magnetic fields; highly resistant to demagnetization, requiring multi-step reversing step-down DC demagnetization cycles.
Summary Comparison Table: Magnetically Soft vs. Hard Materials
- Parameter / Feature Magnetically Soft Materials Magnetically Hard Materials
- Hysteresis Loop Geometry Narrow, tall, slender Wide, broad, squat
Magnetic Permeability ( μ \mu μ ) Very high (typically 1 , 000 1,000 1 , 000 to > 50 , 000 >50,000 > 50 , 000 ) Low to moderate ( 50 50 50 to 500 500 500 )
Coercive Force ( H c H_c H c ) Very low ( < 10 Oe < 10\text{ Oe} < 10 Oe ; often < 2 Oe < 2\text{ Oe} < 2 Oe ) High to very high ( 50 50 50 to > 500 Oe >500\text{ Oe} > 500 Oe )
Retentivity ( B r B_r B r ) Low to moderate; flux decays rapidly High; retains strong persistent field
Hysteresis Energy Loss ( ∮ H d B \oint H dB ∮ H d B ) Minimal heat generation per cycle Substantial heat generation per cycle
- Typical Heat Treatment State Annealed, normalized, low-carbon Quenched and tempered, martensitic, aged
- Representative Materials AISI 1018, ASTM A36, soft iron Quenched 4340, D2 tool steel, 440C
- Continuous MT Sensitivity Optimal (full saturation maintained) High (requires high magnetizing force)
- Residual MT Sensitivity Unacceptable (residual field too weak) Feasible (if permitted by code/spec)
- Demagnetization Demands Effortless; standard AC coil Rigorous; reversing step-down DC
- Continuous vs. Residual Magnetization Techniques
The shape and properties of the B-H curve govern the foundational selection between the Continuous Method and the Residual Method in Magnetic Particle Testing.
The Continuous Method
In the continuous method, magnetic particles (dry powder or wet suspension) are applied to the test surface while the magnetizing current is actively flowing, or the suspension application is ceased immediately prior to current termination.
Physical Mechanism: Inspection takes place at peak magnetic induction ( B B B ), operating near the upper knee or saturation plateau of the B-H curve.
Advantages:
Maximum Sensitivity: Because B B B is maintained at peak operating levels, magnetic flux leakage across tight, shallow, or subsurface flaws is maximized.
Universal Applicability: It is the only reliable method for magnetically soft alloys (low-carbon steels) because their low retentivity causes residual flux to drop precipitously once current stops.
Code Mandate: Major aerospace and structural fabrication codes (e.g., ASTM E1444, ASME Section V Article 7) strictly mandate the continuous method for all primary inspections unless an explicit engineering variance is authorized.
The Residual Method
In the residual method, the component is magnetized by an initial current pulse, the magnetizing current is completely terminated, and magnetic particles are subsequently applied to the surface utilizing only the residual magnetic field ( B r B_r B r ).
Physical Mechanism: Inspection relies entirely on the material's retentivity and coercive force to sustain a leakage field without an active external magnetizing force.
Strict Limitations:
Material Restriction: Can ONLY be utilized on magnetically hard materials possessing high retentivity ( B r B_r B r ) and high coercive force ( H c H_c H c ). If attempted on soft low-carbon steel, the residual field drops below the threshold needed to bridge crack air gaps, yielding false-negative results.
Reduced Sensitivity: Even in hard steels, the residual flux density B r B_r B r is substantially lower than saturation induction B s a t B_{sat} B s a t . Leakage fields are weaker, making the residual method blind to tight micro-cracks and subsurface discontinuities.
Restricted Use Cases: Primarily utilized for automated, high-throughput screening of small, identical, case-hardened fasteners, bearing balls, or heat-treated tool components where suspension pooling under active current might cause excessive background.
Level III Engineering Analysis: Demagnetization Physics
Demagnetization is the systematic reversal and progressive reduction of the B-H hysteresis loop down to the origin ( 0 , 0 ) (0,0) ( 0 , 0 ) .
A high coercive force ( H c H_c H c ) indicates that magnetic domain walls are firmly trapped at microscopic pinning sites.
An inspector attempting to demagnetize a quenched AISI 4340 landing gear cylinder ( H c ≈ 70 Oe H_c \approx 70\text{ Oe} H c ≈ 70 Oe ) with a portable 60 Hz AC pull-through coil will fail: the skin effect confines the 60 Hz field to the outer millimeter of the part, leaving the internal core heavily magnetized, and the peak field intensity of the coil is often insufficient to overcome H c H_c H c .
The Level III must design a demagnetization procedure utilizing low-frequency, reversing step-down direct current (e.g., 0.5 to 1 Hz, 30 to 40 steps, stepping current down from 3,000 Amperes to zero), ensuring full-depth penetration and complete loop collapse.