6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity
AWS API 1104 Pipeline Welding Endorsement Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Overview & Scope of API 1104:2021
1.1 Scope, Definitions & General Requirements 1.2 Base Materials & Filler Metal Groupings
2 Chapter 2: Welding Procedure Qualification (Section 5)
2.1 Welding Procedure Specification (WPS) Requirements & Contents 2.2 Essential Variables for Procedure Qualification (Section 5.4) 2.3 Mechanical Testing Requirements and Specimen Preparation 2.4 Acceptance Criteria for Procedure Qualification
3 Chapter 3: Welder Qualification (Section 6)
3.1 Single Qualification Testing & Essential Variables 3.2 Multiple Qualification Testing & Layout 3.3 Visual & Destructive Test Specimen Layout 3.4 Acceptance Criteria & Retesting Rules for Welders
4 Chapter 4: Design & Fabrication of Pipeline Welds (Section 7)
4.1 Joint Alignment, High-Low & Fit-Up Tolerances 4.2 Preheating, Interpass Temperature & Heat Treatment 4.3 Tack Welding, Line-Up Clamps & Weather Restrictions 4.4 Filler Metal Storage, Handling & Conditioning
5 Chapter 5: Inspection & Non-Destructive Testing (Sections 8 & 11)
5.1 Rights & Responsibilities of Inspection Personnel 5.2 Radiographic Testing (RT) & Image Quality Indicators (IQI) 5.3 Ultrasonic Testing (UT) & Automated UT (AUT/PAUT) 5.4 Magnetic Particle (MT), Liquid Penetrant (PT) & Personnel Qualification
6 Chapter 6: Acceptance Standards for Imperfections (Section 9)
6.1 Inadequate Penetration (IP), IP Due to High-Low (IPD) & Cross Penetration (ICP) 6.2 Incomplete Fusion (IF & IFD), Internal Concavity (IC) & Burn-Through (BT) 6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity 6.4 Porosity — Scattered (P), Distribution Charts & Hollow Bead Cross-Reference 6.5 Undercutting, Crater Cracks & Arc Burns 6.6 Cracks, Accumulation of Imperfections & Annex A (ECA)
7 Chapter 7: Repair, Mechanized Welding & Records (Sections 10 & 12)
7.1 Repair Procedure Qualification & Limitations 7.2 Defect Removal, Grinding & Re-Inspection 7.3 Welding Records, Traceability & Inspector Logs 7.4 Mechanized Welding with Filler Metal Additions (Section 12)
8 Chapter 8: Annex B — In-Service Pipeline Welding
8.1 In-Service Welding Dynamics, Burn-Through & HIC Risks 8.2 Temper-Bead Deposition Techniques & Sequence 8.3 In-Service Procedure & Welder Qualification Requirements
6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity
Key Takeaways Explain This Topic AI
Elongated Slag Inclusions (ESI, 9.3.8) are defects when an individual indication exceeds 2 in. (50 mm), the aggregate exceeds 2 in. per 12 in. (300 mm), or the width exceeds 1/16 in. (1.6 mm).
Parallel ESI "wagon tracks" separated by about the root bead width count as ONE indication unless the width of either exceeds 1/32 in. (0.8 mm) — then they are evaluated separately.
Isolated Slag Inclusions (ISI) are defects when the aggregate exceeds 1/2 in. (13 mm) per 12 in., the width exceeds 1/8 in. (3 mm), or more than four ISI at the maximum 1/8 in. width appear in any 12 in. of weld.
On pipe OD < 2.375 in., ESI individual length is limited to three times the thinner specified wall, and ISI aggregate to two times the thinner wall with width limited to half the wall.
Hollow Bead porosity (HB, 9.3.9.3) — elongated linear porosity in the root bead — is a defect when an individual indication exceeds 1 in. (25 mm), the aggregate exceeds 2 in. (50 mm) per 12 in., or the aggregate exceeds 8% of weld length.
Last updated: August 2026
6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity
Slag inclusions and hollow-bead voids are the everyday volumetric discontinuities of SMAW pipeline welding. API 1104:2021 evaluates slag in Section 9.3.8 and hollow bead in Section 9.3.9.3 . When measuring a radiographic slag indication, its maximum dimension counts as its length.
1. Slag Inclusions (9.3.8) — Large-Diameter Pipe (OD ≥ 2.375 in.)
Elongated Slag Inclusions (ESI) — continuous or broken slag lines ("wagon tracks") at the fusion zone — are defects when:
- an individual ESI indication exceeds 2 in. (50 mm) in length;
- the aggregate length of ESI exceeds 2 in. (50 mm) in any continuous 12 in. (300 mm) of weld; or
the width of an ESI indication exceeds 1/16 in. (1.6 mm) .
Wagon-track rule: parallel ESI lines separated by approximately the width of the root bead are considered a single indication — unless the width of either line exceeds 1/32 in. (0.8 mm) , in which case they are evaluated as separate indications.
Isolated Slag Inclusions (ISI) — irregularly shaped slag pockets anywhere in the weld — are defects when:
- the aggregate length of ISI exceeds 1/2 in. (13 mm) in any continuous 12 in. (300 mm) of weld;
- the width of an ISI indication exceeds 1/8 in. (3 mm) ; or
more than four ISI indications at the maximum 1/8 in. (3 mm) width appear in any continuous 12 in. (300 mm) of weld.
Finally, the aggregate length of ESI and ISI indications together may not exceed 8% of the weld length .
2. Slag Inclusions — Small-Diameter Pipe (OD < 2.375 in.)
ESI: individual length may not exceed three times the thinner specified wall thickness ; width limit stays 1/16 in. (1.6 mm).
ISI: aggregate length may not exceed two times the thinner wall AND width may not exceed one-half the thinner wall .
The 8% aggregate rule still applies.
3. Hollow Bead Porosity — HB (9.3.9.3)
Hollow bead is elongated linear porosity occurring along the root-bead centerline — trapped hydrogen/CO bubbles from fast vertical-down cellulosic root passes. On a radiograph it shows as a smooth, dark, tubular shadow centered in the root bead.
HB is a defect when:
an individual HB indication exceeds 1 in. (25 mm) — note the 22nd edition relaxed this from the 21st edition's 1/2 in.;
the aggregate length of HB exceeds 2 in. (50 mm) in any continuous 12 in. (300 mm) of weld; or
the aggregate length of all HB exceeds 8% of the weld length .
4. Comparison Matrix
- Parameter ESI ISI HB (9.3.9.3)
- Individual length > 2 in. (50 mm) = defect (governed by aggregate/width/count) > 1 in. (25 mm) = defect
- Aggregate per 12 in. > 2 in. (50 mm) = defect > 1/2 in. (13 mm) = defect > 2 in. (50 mm) = defect
- Width > 1/16 in. (1.6 mm) = defect > 1/8 in. (3 mm) = defect n/a
- Count rule Wagon tracks = single unless width > 1/32 in. > 4 at max width per 12 in. = defect n/a
- Short welds ESI+ISI aggregate > 8% of weld length same aggregate > 8% of weld length
- 5. Worked Evaluations
- Scenario A — ESI on 0.375 in. wall, 24 in. OD pipe
One ESI line, 1.25 in. long × 0.040 in. wide. Individual limit is 2.0 in. (there is NO t/2 reduction for radiographic ESI — that reduction belongs to nick-break slag). Width 0.040 ≤ 1/16 in. ACCEPTED , provided the 12 in. aggregate stays ≤ 2.0 in.
Scenario B — ISI count rule
Five ISI indications, each at the maximum 1/8 in. width, in one 12 in. segment, aggregate 0.55 in. Width: at the 1/8 in. limit (OK individually); aggregate: 0.55 > 0.5 in. and more than four at maximum width — REJECTED on two grounds.
Scenario C — HB on a short weld
Weld length 7.5 in. (2.375 in. OD nipple). One HB indication, 0.9 in. Individual: 0.9 ≤ 1.0 in. OK. Aggregate: 0.9 > 8% × 7.5 = 0.60 in. → REJECTED by the 8% rule.
- 6. Causes, Prevention, and Radiographic Recognition
- What the Definitions Anchor
Section 3 defines a slag inclusion as a nonmetallic solid entrapped in the weld metal or between the weld metal and the parent material (3.1.54), and porosity as gas trapped by solidifying weld metal before the gas has a chance to rise to the surface of the molten puddle and escape (3.1.35). Hollow bead is the elongated linear porosity that occurs in the root bead (3.1.18). Per 9.3.8.1, ESIs are usually found at the fusion zone, while ISIs are irregularly shaped and may be located anywhere in the weld.
How They Form — and How Crews Prevent Them
ESI / wagon tracks: slag trapped in the toes alongside an underfilled or crowned root bead when the following pass fails to remelt it and float it out. Prevention: correct bead profile, proper electrode angle and current, and thorough interpass chipping, grinding, or wire-brushing with the power or hand tools the WPS designates (5.3.2.12).
ISI: slag pockets left between passes by incomplete cleaning, excessive weaving that undercuts the bead toes, or slag frozen into the deep valleys of a rough ripple pattern. Prevention: clean every pass to bright metal before depositing the next.
HB: gas — chiefly hydrogen and carbon monoxide generated by cellulosic electrode coatings — entrained along the solidifying centerline of a fast vertical-down root pass. Excessive travel speed, a long arc, moisture, or a contaminated joint face aggravate it. Prevention: qualified travel speed and arc length, dry electrodes and joint faces, and the root-bead sizing the WPS specifies.
Telling Them Apart on Film
ESI images as linear dark lines hugging the fusion-zone edges — often the paired wagon tracks of the single-indication rule. ISI images as irregular, isolated dark spots anywhere in the weld cross-section. HB images as a smooth-walled, tubular dark line centered in the root bead — distinct from the sharp, straight-edged dark line of IP and from the broad, diffuse density change of internal concavity.