8.2 Temper-Bead Deposition Techniques & Sequence

AWS API 1104 Pipeline Welding Endorsement Exam

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: Overview & Scope of API 1104:2021

1.1 Scope, Definitions & General Requirements 1.2 Base Materials & Filler Metal Groupings

2 Chapter 2: Welding Procedure Qualification (Section 5)

2.1 Welding Procedure Specification (WPS) Requirements & Contents 2.2 Essential Variables for Procedure Qualification (Section 5.4) 2.3 Mechanical Testing Requirements and Specimen Preparation 2.4 Acceptance Criteria for Procedure Qualification

3 Chapter 3: Welder Qualification (Section 6)

3.1 Single Qualification Testing & Essential Variables 3.2 Multiple Qualification Testing & Layout 3.3 Visual & Destructive Test Specimen Layout 3.4 Acceptance Criteria & Retesting Rules for Welders

4 Chapter 4: Design & Fabrication of Pipeline Welds (Section 7)

4.1 Joint Alignment, High-Low & Fit-Up Tolerances 4.2 Preheating, Interpass Temperature & Heat Treatment 4.3 Tack Welding, Line-Up Clamps & Weather Restrictions 4.4 Filler Metal Storage, Handling & Conditioning

5 Chapter 5: Inspection & Non-Destructive Testing (Sections 8 & 11)

5.1 Rights & Responsibilities of Inspection Personnel 5.2 Radiographic Testing (RT) & Image Quality Indicators (IQI) 5.3 Ultrasonic Testing (UT) & Automated UT (AUT/PAUT) 5.4 Magnetic Particle (MT), Liquid Penetrant (PT) & Personnel Qualification

6 Chapter 6: Acceptance Standards for Imperfections (Section 9)

6.1 Inadequate Penetration (IP), IP Due to High-Low (IPD) & Cross Penetration (ICP) 6.2 Incomplete Fusion (IF & IFD), Internal Concavity (IC) & Burn-Through (BT) 6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity 6.4 Porosity — Scattered (P), Distribution Charts & Hollow Bead Cross-Reference 6.5 Undercutting, Crater Cracks & Arc Burns 6.6 Cracks, Accumulation of Imperfections & Annex A (ECA)

7 Chapter 7: Repair, Mechanized Welding & Records (Sections 10 & 12)

7.1 Repair Procedure Qualification & Limitations 7.2 Defect Removal, Grinding & Re-Inspection 7.3 Welding Records, Traceability & Inspector Logs 7.4 Mechanized Welding with Filler Metal Additions (Section 12)

8 Chapter 8: Annex B — In-Service Pipeline Welding

8.1 In-Service Welding Dynamics, Burn-Through & HIC Risks 8.2 Temper-Bead Deposition Techniques & Sequence 8.3 In-Service Procedure & Welder Qualification Requirements

8.2 Temper-Bead Deposition Techniques & Sequence

Key Takeaways Explain This Topic AI

Temper-bead welding deposits each subsequent pass so its thermal envelope reheats and tempers the hard, brittle HAZ left by the previous pass — no PWHT possible on a live line.

Annex B distinguishes heat-input control procedures (high enough heat input to overcome the contents' heat removal) from temper-bead procedures (deposition sequence engineered for tempering); the WPS specifies the heat-input range for each layer and the bead sequence with spacing tolerances.

The tempering layer needs enough heat input to reach the underlying HAZ but not so much that it burns through the first layer and creates a new untempered HAZ.

Stringer beads with controlled overlap temper the HAZ continuously; weaving is avoided because it makes heat input and HAZ depth inconsistent.

Consumable discipline is strict: low-hydrogen electrodes (H4/H8 class diffusible hydrogen), sealed containers, holding ovens at 250°F-300°F (120°C-150°C), and rebake or discard after excess atmospheric exposure.

Last updated: August 2026

8.2 Temper-Bead Deposition Techniques & Sequence

Post-weld heat treatment is impossible on an operating hydrocarbon pipeline, so API 1104:2021 Annex B achieves HAZ softening in the weld sequence itself. Temper-bead welding positions and sizes each later pass so its heat reheats — and tempers — the hard HAZ created by the earlier pass. Figure B.1 of the standard shows typical temper-bead deposition sequences.

1. The Metallurgy

A first bead on a cold, flow-cooled pipe wall produces a coarse-grained HAZ (CGHAZ) of untempered martensite — hard and crack-susceptible. A correctly placed second bead pushes a controlled thermal pulse into that CGHAZ. If the CGHAZ reheats into the subcritical tempering range (below the Ac1 transformation temperature):

  • carbon precipitates out of the supersaturated martensite as fine carbides,
  • hardness drops and toughness recovers,

and no new hard HAZ forms, because the second bead's own HAZ lands mostly in the first bead's weld metal.

The window is narrow: too little second-layer heat and the CGHAZ never tempers; too much and the arc penetrates the first layer, re-austenitizing fresh pipe steel and creating a NEW untempered HAZ deeper in the wall. That is why Annex B treats the weld deposition sequence and the heat input range for each layer as specified WPS content (B.2.2.1.3/B.2.2.1.4), with bead-spacing tolerances, and makes sequence changes an essential variable (Table B.1; also 5.4.2.11 for temper-bead techniques generally).

2. Heat-Input Control vs. Temper-Bead Procedures

Annex B recognizes two strategies for overcoming the heat-sink effect of flowing contents:

Strategy How it works WPS content

Heat-input control procedure Heat input high enough to slow cooling despite the flowing contents Required heat-input range

Temper-bead procedure Deposition sequence tempers each prior HAZ Heat-input range for each layer plus the deposition sequence with bead-spacing tolerances

Preheat, where practicable, supplements either strategy — though the contents often make effective preheat difficult to hold.

3. Execution Discipline

Stringer beads only. Weaving makes heat input and HAZ depth irregular; temper-bead work uses tight stringers with precise toe placement.

Overlap control. Adjacent beads overlap by a controlled fraction of bead width (about half) so each new bead tempers its neighbor's HAZ across the whole band.

Layering. The first (buttering) layer uses small electrodes and modest heat input to avoid burning through; the second (tempering) layer runs hotter to push the tempering pulse through the first layer into the pipe HAZ; later fill layers build to size.

Fit-up first. Sleeve/saddle gaps are minimized (weld-metal buildup on the carrier pipe is permitted) to cut restraint stress (B.4.2).

4. Consumable Discipline

Temper-bead control fixes the microstructure leg; hydrogen control fixes the second leg of the triad:

Low-hydrogen consumables — SMAW electrodes to AWS A5.1/A5.5 such as E7018-H4R, or controlled processes — with diffusible hydrogen designators H4 (≤ 4 mL/100 g) or H8 (≤ 8 mL/100 g) .

Storage: factory-sealed containers until use; opened electrodes into holding ovens at 250°F-300°F (120°C-150°C) ; exposure beyond the manufacturer limit (commonly 4 hours, less for high-strength grades in humidity) → rebake per manufacturer (typically 500°F-800°F / 260°C-430°C for 1-2 hours) or discard.

Cellulosic electrodes (E6010/E7010/E8010) produce high diffusible hydrogen and high HAZ hardness — Annex B's Table B.4 hardness limits effectively drive in-service welding to low-hydrogen practice.

5. Where Temper-Bead Fits in Annex B Geometry

Figure B.1's sequences apply to the recurring in-service geometries: full-encirclement sleeves, reinforcing pads and saddles, encirclement tees, and weld-deposition repairs (Figures B.7-B.12 illustrate the fitting configurations). In each case the fillet or groove weld onto the carrier pipe gets the temper-bead treatment: a buttering layer on the pipe surface, a tempering layer over it, then structural fills.

The technique's acceptance is proven in qualification, not assumed: the procedure test assembly (Section 8.3 of this guide) must show the hardness results of Table B.4 across the macrosection. A deposition sequence change after qualification is an essential variable (Table B.1) — the sequence IS the heat treatment, so improvising bead order in the field voids the procedure.

6. Layering Summary

Layer Typical electrode Heat input Function

Buttering (first) Small-diameter low-hydrogen (3/32-1/8 in.) Lower Bond to pipe with minimum penetration — burn-through control

  • Tempering (second) Larger diameter (1/8-5/32 in.) Higher Thermal pulse tempers the buttering layer's CGHAZ
  • Fill/cap Per WPS Per WPS Build to size; each pass continues the tempering chain

The exact electrode sizes, heat inputs, and bead placements are properties of the qualified WPS — the table shows the logic, not universal values.