Study guide
3.1 Single Qualification Testing & Essential Variables
AWS API 1104 Pipeline Welding Endorsement Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Overview & Scope of API 1104:2021
1.1 Scope, Definitions & General Requirements 1.2 Base Materials & Filler Metal Groupings
2 Chapter 2: Welding Procedure Qualification (Section 5)
2.1 Welding Procedure Specification (WPS) Requirements & Contents 2.2 Essential Variables for Procedure Qualification (Section 5.4) 2.3 Mechanical Testing Requirements and Specimen Preparation 2.4 Acceptance Criteria for Procedure Qualification
3 Chapter 3: Welder Qualification (Section 6)
3.1 Single Qualification Testing & Essential Variables 3.2 Multiple Qualification Testing & Layout 3.3 Visual & Destructive Test Specimen Layout 3.4 Acceptance Criteria & Retesting Rules for Welders
4 Chapter 4: Design & Fabrication of Pipeline Welds (Section 7)
4.1 Joint Alignment, High-Low & Fit-Up Tolerances 4.2 Preheating, Interpass Temperature & Heat Treatment 4.3 Tack Welding, Line-Up Clamps & Weather Restrictions 4.4 Filler Metal Storage, Handling & Conditioning
5 Chapter 5: Inspection & Non-Destructive Testing (Sections 8 & 11)
5.1 Rights & Responsibilities of Inspection Personnel 5.2 Radiographic Testing (RT) & Image Quality Indicators (IQI) 5.3 Ultrasonic Testing (UT) & Automated UT (AUT/PAUT) 5.4 Magnetic Particle (MT), Liquid Penetrant (PT) & Personnel Qualification
6 Chapter 6: Acceptance Standards for Imperfections (Section 9)
6.1 Inadequate Penetration (IP), IP Due to High-Low (IPD) & Cross Penetration (ICP) 6.2 Incomplete Fusion (IF & IFD), Internal Concavity (IC) & Burn-Through (BT) 6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity 6.4 Porosity — Scattered (P), Distribution Charts & Hollow Bead Cross-Reference 6.5 Undercutting, Crater Cracks & Arc Burns 6.6 Cracks, Accumulation of Imperfections & Annex A (ECA)
7 Chapter 7: Repair, Mechanized Welding & Records (Sections 10 & 12)
7.1 Repair Procedure Qualification & Limitations 7.2 Defect Removal, Grinding & Re-Inspection 7.3 Welding Records, Traceability & Inspector Logs 7.4 Mechanized Welding with Filler Metal Additions (Section 12)
8 Chapter 8: Annex B — In-Service Pipeline Welding
8.1 In-Service Welding Dynamics, Burn-Through & HIC Risks 8.2 Temper-Bead Deposition Techniques & Sequence 8.3 In-Service Procedure & Welder Qualification Requirements
3.1 Single Qualification Testing & Essential Variables
Key Takeaways Explain This Topic AI
Single qualification (6.2) tests a welder on one test joint in the rolled or fixed position; fixed-position tests may be horizontal, vertical, or inclined not more than 45° from horizontal.
A welder qualified in a fixed position is also qualified for roll welding; a welder qualified only in the roll position may not weld fixed position. Only the 45° inclined fixed test (6G) qualifies butt and lap fillet welds in ALL positions.
OD essential-variable groups: less than 2.375 in. (60.3 mm); 2.375 through 12.750 in. (323.9 mm); greater than 12.750 in.
Qualified thickness range (Table 5): t < 0.154 in. qualifies t to the greater of 0.154 in. or 1.5t; 0.154 ≤ t < 0.750 in. qualifies 0.154 in. to the greater of 0.750 in. or 1.5t; t ≥ 0.750 in. qualifies 0.750 in. to unlimited.
Welder essential variables (6.2.2) include process, direction of welding, Table 4 filler metal group (WF-1 to WF-6), OD group, thickness range, roll-to-fixed position change, joint design, backing elimination, and pass-combination rules; GMAW-S may be used in production only for the same passes used in the qualification test.
Last updated: August 2026
3.1 Single Qualification Testing & Essential Variables
Under API 1104:2021 Section 6.2 , single qualification demonstrates that an individual welder can deposit sound welds under a qualified WPS. The welder welds one test joint — butt, branch, or fillet configuration — and the completed weld must pass visual examination (6.4) plus either destructive testing (6.5) or nondestructive testing (6.6).
1. Test Positions and the Position Hierarchy
For butt-weld single qualification, the welder makes a butt weld in either the rolled or the fixed position. A fixed-position test pipe may be horizontal (5G), vertical (2G), or inclined at not more than 45° from horizontal (6G). The 22nd edition hierarchy:
Fixed position qualifies roll. A welder qualified in any fixed position may also perform roll welding within the qualified variables.
Roll qualifies roll only. A roll-position (1G) qualification does not authorize fixed-position welding.
45° inclined fixed (6G) qualifies everything. A welder who passes a butt weld test in the fixed position with the axis inclined 45° from horizontal is qualified to make butt welds and lap fillet welds in all positions .
A horizontal fixed (5G) or vertical fixed (2G) test qualifies only that fixed position plus roll welding — it does not automatically cover the other fixed positions.
Branch-connection single qualification has its own position matrix (Table 6): the branch test may be run with the branch on the side, top, or bottom of a horizontal run pipe, and the qualified production positions depend on that orientation and the branch/run diameter ratio.
- 2. Qualified Ranges: Outside Diameter and Wall Thickness
- OD Groups (6.2.2 d)
< 2.375 in. (60.3 mm): qualifies only OD less than 2.375 in.
2.375 in. through 12.750 in. (323.9 mm): qualifies that whole band.
> 12.750 in.: qualifies OD ≥ 2.375 in. (all diameters at and above 2.375 in.).
For branch-connection welds, the run pipe diameter is not an essential variable .
Qualified Thickness Range (Table 5)
The 22nd edition replaced the old wall-thickness groups with computed ranges based on the thickness t actually tested:
- Thickness Tested t Qualified Production Thickness Range
- t < 0.154 in. (3.9 mm) t to the greater of 0.154 in. (3.9 mm) or 1.5t
- 0.154 in. ≤ t < 0.750 in. (19 mm) 0.154 in. (3.9 mm) to the greater of 0.750 in. (19 mm) or 1.5t
- t ≥ 0.750 in. (19 mm) 0.750 in. (19 mm) to unlimited
Example: qualifying on 0.375 in. wall covers 0.154-0.750 in. (since 1.5t = 0.562 < 0.750, the 0.750 in. cap governs). Qualifying on 0.500 in. wall covers 0.154-0.750 in. as well (1.5t = 0.750). Qualifying on 0.875 in. wall covers 0.750 in. to unlimited.
For branch connections and lap fillet welds, the run pipe thickness is not an essential variable .
3. Welder Essential Variables (6.2.2)
A change in any of the following requires the welder to requalify:
Welding process — a different process, or a change in the combination of processes (unless each process in the combination was qualified by separate tests).
Direction of welding — vertical up ↔ vertical down, or vertical ↔ horizontal progression. (Welding across the 12 or 6 o'clock positions of a horizontal pipe to avoid stacking starts/stops is not a direction change.)
Filler metal — a change of filler metal group in Table 4 (WF-1 cellulosic SMAW; WF-2 low-hydrogen SMAW; WF-3 low-hydrogen vertical-down SMAW; WF-4 solid-wire GMAW/GTAW; WF-5 oxyfuel; WF-6 FCAW), or a change involving a classification not listed in Table 4.
OD group and thickness range — outside the qualified bands above.
Roll ↔ fixed position , or a change in welding position beyond the hierarchy above.
Joint design — a change per Note e of Table 1 (major joint type). A welder qualified on a butt weld may also make fillet welds within the qualified variables.
Backing — elimination of a backing strip or weld-metal backing.
Pass combination — when multiple processes complete a joint, a change in which passes each process welds. A fill/cap process may be used for a complete production weld only if it ran three or more passes in the test; a process used for fewer than three test passes may weld no more than two production passes.
GMAW-S restriction — with short-circuiting gas metal arc welding, the welder may use GMAW-S in production only for the same passes welded with GMAW-S in the qualification test.