Study guide
2.4 Acceptance Criteria for Procedure Qualification
AWS API 1104 Pipeline Welding Endorsement Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Overview & Scope of API 1104:2021
1.1 Scope, Definitions & General Requirements 1.2 Base Materials & Filler Metal Groupings
2 Chapter 2: Welding Procedure Qualification (Section 5)
2.1 Welding Procedure Specification (WPS) Requirements & Contents 2.2 Essential Variables for Procedure Qualification (Section 5.4) 2.3 Mechanical Testing Requirements and Specimen Preparation 2.4 Acceptance Criteria for Procedure Qualification
3 Chapter 3: Welder Qualification (Section 6)
3.1 Single Qualification Testing & Essential Variables 3.2 Multiple Qualification Testing & Layout 3.3 Visual & Destructive Test Specimen Layout 3.4 Acceptance Criteria & Retesting Rules for Welders
4 Chapter 4: Design & Fabrication of Pipeline Welds (Section 7)
4.1 Joint Alignment, High-Low & Fit-Up Tolerances 4.2 Preheating, Interpass Temperature & Heat Treatment 4.3 Tack Welding, Line-Up Clamps & Weather Restrictions 4.4 Filler Metal Storage, Handling & Conditioning
5 Chapter 5: Inspection & Non-Destructive Testing (Sections 8 & 11)
5.1 Rights & Responsibilities of Inspection Personnel 5.2 Radiographic Testing (RT) & Image Quality Indicators (IQI) 5.3 Ultrasonic Testing (UT) & Automated UT (AUT/PAUT) 5.4 Magnetic Particle (MT), Liquid Penetrant (PT) & Personnel Qualification
6 Chapter 6: Acceptance Standards for Imperfections (Section 9)
6.1 Inadequate Penetration (IP), IP Due to High-Low (IPD) & Cross Penetration (ICP) 6.2 Incomplete Fusion (IF & IFD), Internal Concavity (IC) & Burn-Through (BT) 6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity 6.4 Porosity — Scattered (P), Distribution Charts & Hollow Bead Cross-Reference 6.5 Undercutting, Crater Cracks & Arc Burns 6.6 Cracks, Accumulation of Imperfections & Annex A (ECA)
7 Chapter 7: Repair, Mechanized Welding & Records (Sections 10 & 12)
7.1 Repair Procedure Qualification & Limitations 7.2 Defect Removal, Grinding & Re-Inspection 7.3 Welding Records, Traceability & Inspector Logs 7.4 Mechanized Welding with Filler Metal Additions (Section 12)
8 Chapter 8: Annex B — In-Service Pipeline Welding
8.1 In-Service Welding Dynamics, Burn-Through & HIC Risks 8.2 Temper-Bead Deposition Techniques & Sequence 8.3 In-Service Procedure & Welder Qualification Requirements
2.4 Acceptance Criteria for Procedure Qualification
Key Takeaways Explain This Topic AI
Tensile acceptance (5.6.2.3): weld strength must be ≥ the pipe's specified minimum TENSILE strength (SMTS) — not SMYS; a specimen breaking in the parent metal at ≥ 95% of SMTS is accepted.
When welding materials of different grades, the SMTS of the LOWER grade is the acceptance criterion.
Nick-break acceptance (5.6.3.3): complete penetration and fusion; individual gas pockets ≤ 1/16 in. (1.6 mm); combined gas-pocket area ≤ 2% of the exposed surface; slag inclusions ≤ 1/32 in. (0.8 mm) deep and ≤ 1/8 in. (3 mm) or half the wall in length, separated by ≥ 1/2 in. (13 mm); fisheyes are not cause for rejection.
Bend acceptance (5.6.4.3): no crack or open flaw exceeding 1/8 in. (3 mm) or half the wall thickness in any direction; corner cracks under 1/4 in. (6 mm) are disregarded unless they contain obvious imperfections.
Branch and fillet procedure welds (5.8) are tested with at least four nick-break specimens broken in the weld and evaluated to the same soundness limits — not by macro-etch.
Last updated: August 2026
2.4 Acceptance Criteria for Procedure Qualification
A candidate WPS is qualified only when every destructive specimen satisfies the acceptance requirements of API 1104:2021 Section 5.6 (butt welds) or 5.8 (branch and fillet welds) . This section gives the exact thresholds and the worked calculations the endorsement exam favors.
1. Tensile Test Acceptance (5.6.2.3)
The specimen is pulled to failure and tensile strength S = maximum load ÷ smallest original cross-sectional area. Acceptance compares strength to the pipe's Specified Minimum TENSILE Strength (SMTS) — a critical 22nd-edition detail:
Break in the weld or fusion zone: acceptable if the observed strength is ≥ the SMTS of the pipe material AND the fracture meets the nick-break soundness requirements of 5.6.3.3.
Break in the parent metal (outside weld and HAZ): acceptable if strength is ≥ 95% of SMTS .
Break in the weld below SMTS: the weld is set aside and a new test weld is made.
Different grades in one joint: the lower grade's SMTS governs.
Critical exam distinction: the comparison value is the pipe specification's minimum TENSILE strength (e.g., API 5L X65 → SMTS 77,600 psi), never the yield strength (SMYS) and never the material's actual measured tensile strength. A weld break between SMYS and SMTS FAILS.
Worked Example (X65, SMTS = 77,600 psi)
Reduced-section straps 1.000 in. wide × 0.375 in. thick → area A = 0.375 in.².
Specimen A (weld-metal fracture), P = 29,250 lbf: S = 29,250 / 0.375 = 78,000 psi ≥ 77,600 psi → PASSES .
Specimen B (parent-metal fracture), P = 28,125 lbf: S = 75,000 psi; threshold = 0.95 × 77,600 = 73,720 psi → 75,000 ≥ 73,720 → PASSES (weld shows no internal defects).
Specimen C (weld-metal fracture), P = 27,000 lbf: S = 72,000 psi < 77,600 psi → FAILS ; a new test weld is required.
2. Nick-Break Acceptance (5.6.3.3)
The exposed fracture surfaces of each nick-break specimen are examined for soundness:
Complete penetration and fusion across the root and between passes — zero tolerance for lack of penetration or lack of fusion.
Gas pockets: greatest dimension of any single pocket ≤ 1/16 in. (1.6 mm) ; combined area of all gas pockets ≤ 2% of the exposed surface area .
Slag inclusions: depth ≤ 1/32 in. (0.8 mm) ; length ≤ 1/8 in. (3 mm) or one-half the specified wall thickness, whichever is smaller ; adjacent inclusions separated by at least 1/2 in. (13 mm) of sound metal.
Fisheyes (per AWS A3.0) are not cause for rejection.
3. Guided-Bend Acceptance (5.6.4.3 / 5.6.5.3)
Root, face, and side bends are bent in the Figure 8 jig (plunger radius 1-3/4 in., die radius 2-5/16 in.):
No crack or other imperfection exceeding 1/8 in. (3 mm) or one-half the specified wall thickness, whichever is smaller , in any direction, in the weld or at the fusion zone after bending.
Corner-crack exception: cracks originating on the outer bend radius along the specimen edges, measuring less than 1/4 in. (6 mm) in any direction, are disregarded unless obvious imperfections are observed in them.
4. Branch and Fillet Welds (5.7-5.8)
Branch and fillet procedure test joints are not tensile or bend tested. Section 5.8 requires at least four nick-break specimens cut from the joint at the Figure 10/11 locations (approximately 90° apart, covering crotch and saddle areas), each broken in the weld and evaluated to the same soundness limits as 5.6.3.3: complete penetration and fusion, gas pockets ≤ 1/16 in. with combined area ≤ 2%, slag ≤ 1/32 in. deep and ≤ 1/8 in. or t/2 long, and ≥ 1/2 in. separation. For pipe under 2.375 in. OD, two test welds may be needed (two specimens from each).
5. Single-Specimen Failure and Replacement Rules
The 22nd edition handles isolated specimen failures narrowly:
Improper preparation or testing: a specimen that fails due to improper specimen preparation or testing may be replaced and retested (any test type).
Nick-break, root/face bend, or side bend on test welds over 12-3/4 in. (323.9 mm) OD: if only ONE specimen fails, the company may either reject the weld or replace it with two additional specimens cut as close as possible to (adjacent to) the failed location. Both replacements must pass ; if either fails, the weld is unacceptable.
Tensile break in the weld below SMTS: no specimen replacement — a new test weld is required.