Study guide
2.3 Mechanical Testing Requirements and Specimen Preparation
AWS API 1104 Pipeline Welding Endorsement Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Overview & Scope of API 1104:2021
1.1 Scope, Definitions & General Requirements 1.2 Base Materials & Filler Metal Groupings
2 Chapter 2: Welding Procedure Qualification (Section 5)
2.1 Welding Procedure Specification (WPS) Requirements & Contents 2.2 Essential Variables for Procedure Qualification (Section 5.4) 2.3 Mechanical Testing Requirements and Specimen Preparation 2.4 Acceptance Criteria for Procedure Qualification
3 Chapter 3: Welder Qualification (Section 6)
3.1 Single Qualification Testing & Essential Variables 3.2 Multiple Qualification Testing & Layout 3.3 Visual & Destructive Test Specimen Layout 3.4 Acceptance Criteria & Retesting Rules for Welders
4 Chapter 4: Design & Fabrication of Pipeline Welds (Section 7)
4.1 Joint Alignment, High-Low & Fit-Up Tolerances 4.2 Preheating, Interpass Temperature & Heat Treatment 4.3 Tack Welding, Line-Up Clamps & Weather Restrictions 4.4 Filler Metal Storage, Handling & Conditioning
5 Chapter 5: Inspection & Non-Destructive Testing (Sections 8 & 11)
5.1 Rights & Responsibilities of Inspection Personnel 5.2 Radiographic Testing (RT) & Image Quality Indicators (IQI) 5.3 Ultrasonic Testing (UT) & Automated UT (AUT/PAUT) 5.4 Magnetic Particle (MT), Liquid Penetrant (PT) & Personnel Qualification
6 Chapter 6: Acceptance Standards for Imperfections (Section 9)
6.1 Inadequate Penetration (IP), IP Due to High-Low (IPD) & Cross Penetration (ICP) 6.2 Incomplete Fusion (IF & IFD), Internal Concavity (IC) & Burn-Through (BT) 6.3 Slag Inclusions (ESI & ISI) & Hollow Bead (HB) Porosity 6.4 Porosity — Scattered (P), Distribution Charts & Hollow Bead Cross-Reference 6.5 Undercutting, Crater Cracks & Arc Burns 6.6 Cracks, Accumulation of Imperfections & Annex A (ECA)
7 Chapter 7: Repair, Mechanized Welding & Records (Sections 10 & 12)
7.1 Repair Procedure Qualification & Limitations 7.2 Defect Removal, Grinding & Re-Inspection 7.3 Welding Records, Traceability & Inspector Logs 7.4 Mechanized Welding with Filler Metal Additions (Section 12)
8 Chapter 8: Annex B — In-Service Pipeline Welding
8.1 In-Service Welding Dynamics, Burn-Through & HIC Risks 8.2 Temper-Bead Deposition Techniques & Sequence 8.3 In-Service Procedure & Welder Qualification Requirements
2.3 Mechanical Testing Requirements and Specimen Preparation
Key Takeaways Explain This Topic AI
API 1104:2021 Table 3 sets procedure-qualification specimen counts by pipe OD and wall thickness: 4 total for OD ≤ 2.375 in. and for 2.375-4.500 in.; 8 for > 4.500-12.750 in.; 16 for OD > 12.750 in. (two test joints needed below 2.375 in. OD).
For wall thickness over 0.500 in. (12.7 mm), side bends replace root and face bends: 4 side bends at ≤ 4.500 in. OD, 4 at > 4.500-12.750 in., and 8 above 12.750 in.
Nick-break tests may be waived when the procedure weld is examined by radiography or UT and found acceptable per Section 9; for materials with nominal SMYS greater than X42, at least one tensile test is required.
Nick-break specimens are approximately 9 in. × 1 in., notched approximately 1/8 in. (3 mm) deep on each side at the weld centerline.
The guided-bend jig (Figure 8) uses a plunger radius of 1-3/4 in. (45 mm) and a die radius of 2-5/16 in. (60 mm); the company specifies bend radii not greater than Figure 8.
Last updated: August 2026
2.3 Mechanical Testing Requirements and Specimen Preparation
Once a procedure qualification test joint has been welded, it is cut into destructive-test specimens per Section 5.6 and Table 3 of API 1104:2021. Destructive testing verifies tensile strength, internal soundness, and ductility of the joint before the WPS may be used in production.
Specimen Counts — Table 3 (22nd Edition)
Counts depend on pipe outside diameter AND on whether wall thickness exceeds 0.500 in. (12.7 mm):
Pipe OD Wall ≤ 0.500 in. Wall > 0.500 in.
< 2.375 in. (60.3 mm) 2 nick-break + 2 root bend = 4 (one nick-break and one root bend from each of TWO test joints; OD ≤ 1.315 in. may use one full-section tensile) (≤ 4.500 in.) 2 nick-break + 2 side bend = 4
2.375 to 4.500 in. 2 nick-break + 2 root bend = 4 2 nick-break + 2 side bend = 4
> 4.500 to 12.750 in. 2 tensile + 2 nick-break + 2 root bend + 2 face bend = 8 2 tensile + 2 nick-break + 4 side bend = 8
> 12.750 in. (323.9 mm) 4 tensile + 4 nick-break + 4 root bend + 4 face bend = 16 4 tensile + 4 nick-break + 8 side bend = 16
Three Table 3 footnotes are exam favorites:
(a) For materials with nominal SMYS greater than Grade X42, a minimum of one tensile test is required.
(b) Nick-break tests are not required when the procedure weld is examined by radiography or ultrasonic testing and found acceptable per Section 9 — but if the RT/UT result is unacceptable, the procedure is rejected.
(c) Below 2.375 in. OD, two test joints are made to obtain the required specimens; at or below 1.315 in. (33.4 mm) OD, one full-section tensile specimen may be tested instead.
Specimens are removed at equally spaced locations around the circumference (Figure 3), may be rotated at the company's option provided equal spacing, and never include the pipe's longitudinal seam weld. All specimens are air-cooled to ambient temperature before testing.
Specimen Geometry and Preparation
Tensile (5.6.2): full-thickness strap, full-section or reduced-section per Figure 4; weld reinforcement may be removed. Tensile strength = maximum load ÷ smallest cross-sectional area measured before loading.
Nick-break (5.6.3): approximately 9 in. (230 mm) long × 1 in. (25 mm) wide , notched on each side at the weld centerline approximately 1/8 in. (3 mm) deep , edges smooth and parallel. Broken by pulling, bending, or striking; the exposed fracture must be at least 3/4 in. (19 mm) wide. For mechanized/semiautomatic welds prone to breaking through the pipe instead of the weld, the external reinforcement may be notched up to 1/16 in. (1.6 mm) from the original weld surface.
Root/face bend (5.6.4): approximately 9 in. × 1 in.; long edges rounded; cover and root reinforcement removed flush; surfaces smooth with any scratches light and transverse to the weld; never flattened before testing.
Side bend (5.6.5): approximately 9 in. long × 1/2 in. (13 mm) wide (cut oversize then machined to width); reinforcement removed flush.
Guided-Bend Jig (Figure 8)
Bend specimens are forced into a U-shape in a guided-bend jig whose radii are fixed by the standard : plunger radius 1-3/4 in. (45 mm) , die radius 2-5/16 in. (60 mm) , die width 2 in. (50 mm). The company specifies the fixture and bend radii, which may not exceed the Figure 8 radii.
Additional Rules Candidates Miss
Small pipe needs two joints. For pipe under 2.375 in. (60.3 mm) OD, two test joints are welded to obtain the required specimens — one nick-break and one root bend from each. At or below 1.315 in. (33.4 mm) OD, a single full-section tensile specimen may replace them.
Location discipline. Specimens come from the Figure 3 locations; the company may rotate the locations provided they remain equally spaced around the circumference, and specimens never include the pipe's longitudinal seam weld.
Cooling before testing. All specimens are air-cooled to ambient temperature before testing — no quenching to speed the lab schedule.
Macroetch option. At the company's option, nick-break specimens for semiautomatic or mechanized procedure qualifications may be macroetched before being nicked (5.6.3.1 Note 2), exposing the weld profile before fracture.
Hardness/toughness additions. When the company specifies hardness or toughness requirements (Category II), it also specifies the specimen preparation, testing, and acceptance criteria for those measurements.