Study guide
4.2 Impact Testing Requirements & Toughness Thickness Qualification Ranges
AWS ASME BPVC Section IX + B31.1/B31.3 Endorsement CWI/SCWI
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Exam Structure, Logistics & Code Navigation Strategy
1.1 Credential Overview, Prometric Delivery & July 2025 Hard-Copy Rule 1.2 The Three-Code Triad: Section IX, B31.1, and B31.3 Roles & Interrelationships 1.3 Rapid Code-Book Navigation: Tabbing, Cross-Referencing & Time Management
2 Chapter 2: Section IX Article I — General Welding Requirements
2.1 Scope, Responsibilities & Section IX Architecture 2.2 Mechanical Test Types, Specimen Dimensions & Acceptance Criteria 2.3 Notch-Toughness Tests, Fillet-Weld Tests & Special Examinations
3 Chapter 3: Section IX Article II — Procedure Qualification Fundamentals
3.1 PQR vs. WPS Workflow, Purpose & Content Requirements 3.2 Coupling and Supporting Multiple WPSs and PQRs 3.3 Test Coupons, Preparation & Required Test Specimen Allocations
4 Chapter 4: Section IX Procedure Qualification Limits & Thickness Rules
4.1 Base Metal & Deposited Weld Metal Thickness Limits 4.2 Impact Testing Requirements & Toughness Thickness Qualification Ranges 4.3 Fillet Weld Procedure Qualification Rules & Special Applications
5 Chapter 5: Section IX Article III — Welder Performance Qualification Fundamentals
5.1 Welder & Welding Operator Qualification Intent, Responsibilities & Identification 5.2 Qualification Testing Methods: Mechanical Bend Tests vs. Volumetric NDE 5.3 Welder Qualification Continuity, Expiration, and Requalification
6 Chapter 6: Section IX Welder Performance Limits, Positions & Diameters
6.1 Test Positions, Groove Weld Orientations & Production Position Limits 6.2 Welder Thickness Limits and Pipe Diameter Qualification Ranges 6.3 Welder Essential Variables: F-Numbers, Backing, and Process Transfers
7 Chapter 7: Section IX Article IV — Welding Variables by Process (Part 1: SMAW & GTAW)
7.1 Understanding Essential, Supplementary Essential & Nonessential Variables 7.2 Shielded Metal Arc Welding (SMAW) Procedure Variables 7.3 Gas Tungsten Arc Welding (GTAW) Procedure Variables
8 Chapter 8: Section IX Article IV — Welding Variables by Process (Part 2: GMAW/FCAW & SAW)
8.1 GMAW & FCAW Procedure Variables and Short-Circuiting Transfer Rules 8.2 Submerged Arc Welding (SAW) Procedure Variables and Flux-Wire Combinations 8.3 Special Variables: Heat Input, Electrical Characteristics & Shielding Gases
9 Chapter 9: Section IX Material Classifications, Numbers & Standard Documentation
9.1 Base Metal P-Numbers, Group Numbers, and S-Numbers 9.2 Filler Metal F-Numbers and As-Deposited Chemistry A-Numbers 9.3 ASME Standard Documentation: Auditing WPS, PQR, and WPQ Forms
10 Chapter 10: ASME B31.1 Power Piping — Scope, Materials, Design & Welding Fabrication
10.1 B31.1 Scope, Jurisdiction, Boiler External Piping vs. Non-Boiler External Piping 10.2 B31.1 Welding Requirements, Joint Alignment, Backing Rings & Tack Welds 10.3 B31.1 Welder & Procedure Qualification Interfacing with Section IX 10.4 B31.1 Materials, Design Conditions & Pressure Design of Components
11 Chapter 11: ASME B31.1 Power Piping — Heat Treatment, Examination, Testing & Fabrication Records
11.1 B31.1 Preheat Rules & Mandatory Temperatures 11.2 B31.1 Postweld Heat Treatment (PWHT) Rules, Temperatures & Holding Times 11.3 B31.1 Mandatory NDE Examination, Acceptance Standards & Pressure Leak Tests 11.4 B31.1 Bending, Forming, Assembly & Code Records
12 Chapter 12: ASME B31.3 Process Piping — Scope, Fluid Services, Materials, Design & Welding
12.1 B31.3 Scope, Fluid Service Classifications & Owner Responsibilities 12.2 B31.3 Welding, Joint Preparation, Backing Rings & Fabrication Details 12.3 B31.3 Procedure & Performance Qualification Rules and Section IX Exceptions 12.4 B31.3 Materials, Design Conditions & Pressure Design of Components
13 Chapter 13: ASME B31.3 Process Piping — Heat Treatment, Examination, Testing, Fabrication & Records
13.1 B31.3 Preheat and Postweld Heat Treatment Rules & Tables 13.2 B31.3 Inspection vs. Examination Responsibilities & Examination Extents 13.3 B31.3 Acceptance Criteria for Weld Imperfections 13.4 B31.3 Pressure Leak Testing: Hydrostatic, Pneumatic & Sensitive Leak Tests 13.5 B31.3 Bending, Forming, Assembly & Records
4.2 Impact Testing Requirements & Toughness Thickness Qualification Ranges
Key Takeaways Explain This Topic AI
ASME Section IX does not independently mandate Charpy V-notch impact testing; toughness testing requirements and supplementary essential variables are triggered solely by referencing construction codes like ASME Section VIII, B31.1, or B31.3.
Under paragraph QW-403.6, when impact testing is required, the minimum qualified base metal thickness is the lesser of coupon thickness T or 5/8 in. (16 mm), except that for T < 1/4 in. (6 mm), the minimum qualified thickness is 0.5T.
Paragraph QW-403.6 strictly overrides Table QW-451.1 for minimum base metal thickness, preventing procedures qualified on thick plates from qualifying thin materials where high cooling rates and microstructure shifts degrade HAZ toughness.
Heat input calculation per QW-409.1 (H = [V * A * 60] / [Travel Speed * 1000] kJ/in) is a supplementary essential variable; an increase in heat input slows cooling, coarsening HAZ grain structure and severely reducing absorbed impact energy.
Postweld heat treatment (PWHT) holding time under QW-407.2 requires the PQR coupon to undergo at least 80% of the total aggregate PWHT time planned for production fabrication to account for thermal degradation.
Last updated: September 2026
4.2 Impact Testing Requirements & Toughness Thickness Qualification Ranges
Core Principle: ASME Section IX is a testing standard, not a construction code. It does not establish design service temperatures or dictate when Charpy V-notch impact testing is required. However, when a referencing construction code (such as ASME Section VIII Div 1, ASME B31.1, or ASME B31.3) mandates toughness testing, all supplementary essential variables become legally binding essential variables. Under QW-403.6 , standard minimum thickness rules are superseded by strict lower-bound limits designed to preserve heat-affected zone (HAZ) toughness.
1. The Referencing Code Trigger & Supplementary Essential Variables
Paragraph QW-401.3 establishes that supplementary essential variables become active only when notch-toughness testing is specified by the referencing code or engineering design document.
Without Impact Testing: The procedure qualification requires only transverse tension tests (QW-150) and guided-bend tests (QW-160) to evaluate ultimate tensile strength and gross ductility.
With Impact Testing: The procedure must also evaluate dynamic fracture toughness at a designated design minimum temperature using Charpy V-notch specimens (QW-170). In addition, variables that govern weld thermal cycles—specifically heat input, bead width, preheat decrease, interpass increase, and postweld heat treatment time—shift from nonessential status to legally binding essential variables. +-----------------------------------------------------------------------------------------+
- | THE TOUGHNESS QUALIFICATION ARCHITECTURE |
- +-----------------------------------------------------------------------------------------+
- | REFERENCING CODE (B31.1 / B31.3 / SEC VIII) |
- | - Sets Minimum Design Metal Temperature (MDMT) |
- | - Mandates Charpy V-notch testing on Weld Metal and HAZ |
- | - Establishes minimum energy acceptance values (e.g., 15 ft-lbs / 20 Joules) |
- | | |
- | V |
- | ASME SECTION IX (ARTICLE II & IV) |
- | - Activates Supplementary Essential Variables in QW-250 tables |
- | - Enforces QW-403.6 (Restricted minimum base metal thickness) |
- | - Enforces QW-409.1 (Maximum heat input and weld bead volume limits) |
- | - Enforces QW-407.2 (80% PWHT aggregate time-at-temperature rule) |
- +-----------------------------------------------------------------------------------------+
- 2. Minimum Base Metal Thickness Qualified: Paragraph QW-403.6
In non-toughness procedures, Table QW-451.1 allows very broad base metal qualification ranges. For example, a coupon welded on 1.0 in. 1.0\text{ in.} 1.0 in. plate qualifies base metal down to 3 / 16 in. 3/16\text{ in.} 3/16 in. ( 0.1875 in. 0.1875\text{ in.} 0.1875 in. ). However, when notch-toughness testing is invoked, this broad range is legally prohibited.
The Governing Language of QW-403.6
Paragraph QW-403.6 states:
"The minimum base metal thickness qualified is the thickness of the test coupon T T T or 5 / 8 in. 5/8\text{ in.} 5/8 in. ( 16 mm 16\text{ mm} 16 mm ), whichever is less. However, where T T T is less than 1 / 4 in. 1/4\text{ in.} 1/4 in. ( 6 mm 6\text{ mm} 6 mm ), the minimum thickness qualified is 1 / 2 T 1/2T 1/2 T ."
This creates a three-tier rule for minimum base metal thickness:
Coupons Thicker Than 5 / 8 in. 5/8\text{ in.} 5/8 in. ( T ≥ 0.625 in. T \ge 0.625\text{ in.} T ≥ 0.625 in. ):
Qualified minimum thickness is 5 / 8 in. 5/8\text{ in.} 5/8 in. ( 16 mm 16\text{ mm} 16 mm ) .
Example: A 1.5 in. 1.5\text{ in.} 1.5 in. coupon qualifies from 5 / 8 in. 5/8\text{ in.} 5/8 in. ( 0.625 in. 0.625\text{ in.} 0.625 in. ) to 8.0 in. 8.0\text{ in.} 8.0 in. , NOT from 3 / 16 in. 3/16\text{ in.} 3/16 in. !
Coupons from 1 / 4 in. 1/4\text{ in.} 1/4 in. to 5 / 8 in. 5/8\text{ in.} 5/8 in. ( 0.250 in. ≤ T < 0.625 in. 0.250\text{ in.} \le T < 0.625\text{ in.} 0.250 in. ≤ T < 0.625 in. ):
Qualified minimum thickness is T T T (the full coupon thickness).
Example: A 1 / 2 in. 1/2\text{ in.} 1/2 in. ( 0.500 in. 0.500\text{ in.} 0.500 in. ) coupon qualifies from 0.500 in. 0.500\text{ in.} 0.500 in. to 1.000 in. 1.000\text{ in.} 1.000 in. , NOT from 3 / 16 in. 3/16\text{ in.} 3/16 in. !
Coupons Thinner Than 1 / 4 in. 1/4\text{ in.} 1/4 in. ( T < 0.250 in. T < 0.250\text{ in.} T < 0.250 in. ):
Qualified minimum thickness is 0.5 T 0.5T 0.5 T (half the coupon thickness).
Example: A 0.200 in. 0.200\text{ in.} 0.200 in. coupon qualifies from 0.100 in. 0.100\text{ in.} 0.100 in. to 0.400 in. 0.400\text{ in.} 0.400 in. , NOT from 1 / 16 in. 1/16\text{ in.} 1/16 in. !
Coupon Thickness T T T Standard QW-451.1 Min Thickness QW-403.6 Impact-Tested Min Thickness Maximum Base Metal Qualified
0.125 in. 0.125\text{ in.} 0.125 in. ( 1 / 8 in. 1/8\text{ in.} 1/8 in. ) 0.0625 in. 0.0625\text{ in.} 0.0625 in. ( 1 / 16 in. 1/16\text{ in.} 1/16 in. ) 0.0625 in. 0.0625\text{ in.} 0.0625 in. ( 0.5 T 0.5T 0.5 T ) 0.250 in. 0.250\text{ in.} 0.250 in. ( 2 T 2T 2 T )
0.200 in. 0.200\text{ in.} 0.200 in. 0.0625 in. 0.0625\text{ in.} 0.0625 in. ( 1 / 16 in. 1/16\text{ in.} 1/16 in. ) 0.1000 in. 0.1000\text{ in.} 0.1000 in. ( 0.5 T 0.5T 0.5 T ) 0.400 in. 0.400\text{ in.} 0.400 in. ( 2 T 2T 2 T )
0.375 in. 0.375\text{ in.} 0.375 in. ( 3 / 8 in. 3/8\text{ in.} 3/8 in. ) 0.0625 in. 0.0625\text{ in.} 0.0625 in. ( 1 / 16 in. 1/16\text{ in.} 1/16 in. ) 0.3750 in. 0.3750\text{ in.} 0.3750 in. ( T T T ) 0.750 in. 0.750\text{ in.} 0.750 in. ( 2 T 2T 2 T )
0.500 in. 0.500\text{ in.} 0.500 in. ( 1 / 2 in. 1/2\text{ in.} 1/2 in. ) 0.1875 in. 0.1875\text{ in.} 0.1875 in. ( 3 / 16 in. 3/16\text{ in.} 3/16 in. ) 0.5000 in. 0.5000\text{ in.} 0.5000 in. ( T T T ) 1.000 in. 1.000\text{ in.} 1.000 in. ( 2 T 2T 2 T )
0.750 in. 0.750\text{ in.} 0.750 in. ( 3 / 4 in. 3/4\text{ in.} 3/4 in. ) 0.1875 in. 0.1875\text{ in.} 0.1875 in. ( 3 / 16 in. 3/16\text{ in.} 3/16 in. ) 0.6250 in. 0.6250\text{ in.} 0.6250 in. ( 5 / 8 in. 5/8\text{ in.} 5/8 in. ) 1.500 in. 1.500\text{ in.} 1.500 in. ( 2 T 2T 2 T )
1.500 in. 1.500\text{ in.} 1.500 in. ( 1 - 1 / 2 in. 1\text{-}1/2\text{ in.} 1 - 1/2 in. ) 0.1875 in. 0.1875\text{ in.} 0.1875 in. ( 3 / 16 in. 3/16\text{ in.} 3/16 in. ) 0.6250 in. 0.6250\text{ in.} 0.6250 in. ( 5 / 8 in. 5/8\text{ in.} 5/8 in. ) 8.000 in. 8.000\text{ in.} 8.000 in. ( 200 mm 200\text{ mm} 200 mm )
Metallurgical Rationale: The Quench-and-Temper Cooling Effect
Why does Section IX restrict the minimum thickness when impact testing is required? In thick plates, the vast volume of cold steel acts as a massive heat sink, rapidly quenching the weld and HAZ. When welding thin sheet or plate ( < 5 / 8 in. < 5/8\text{ in.} < 5/8 in. ), the heat cannot dissipate into the body of the material as rapidly, resulting in a significantly slower cooling rate ( t 8 / 5 t_{8/5} t 8/5 ) or, conversely, if welded with very low heat, an extreme cooling rate that promotes brittle martensite formation. More critically, high heat input per unit thickness in thin sections leads to substantial thermal saturation and severe grain coarsening in the HAZ. Coarse grain microstructures exhibit dramatically higher ductile-to-brittle transition temperatures (DBTT), causing catastrophic brittle failure under impact loading.
Loading diagram... Figure 4.2: ASME Section IX Notch-Toughness Thickness Qualification Decision Tree (QW-403.6)
3. Heat Input Determination & Cooling Rate Controls: Paragraph QW-409.1
When notch toughness is required, heat input becomes a strictly monitored supplementary essential variable under paragraph QW-409.1 :
The Rule: An increase in heat input, or an increase in the volume of weld metal deposited per unit length of weld bead, over that qualified on the PQR is prohibited without requalification.
The Mathematical Formula for Heat Input
ASME Section IX defines heat input mathematically as: Heat Input ( J / in. ) = Voltage ( V ) × Amperage ( A ) × 60 Travel Speed ( S , inches per minute ) \text{Heat Input } (J/\text{in.}) = \frac{\text{Voltage } (V) \times \text{Amperage } (A) \times 60}{\text{Travel Speed } (S, \text{ inches per minute})} Heat Input ( J / in. ) = Travel Speed ( S , inches per minute ) Voltage ( V ) × Amperage ( A ) × 60
To express heat input in kilojoules per inch ( kJ/in. \text{kJ/in.} kJ/in. ): Heat Input ( kJ/in. ) = V × A × 60 S × 1000 = V × A × 0.06 S \text{Heat Input } (\text{kJ/in.}) = \frac{V \times A \times 60}{S \times 1000} = \frac{V \times A \times 0.06}{S} Heat Input ( kJ/in. ) = S × 1000 V × A × 60 = S V × A × 0.06
In metric units ( kJ/mm \text{kJ/mm} kJ/mm with travel speed in mm/min \text{mm/min} mm/min ): Heat Input ( kJ/mm ) = V × A × 0.06 S ( mm/min ) \text{Heat Input } (\text{kJ/mm}) = \frac{V \times A \times 0.06}{S (\text{mm/min})} Heat Input ( kJ/mm ) = S ( mm/min ) V × A × 0.06
Volume of Weld Metal Deposited per Unit Length
For manual processes (such as SMAW or GTAW) where travel speed may vary considerably, QW-409.1 provides an alternative method of control: weld bead volume per unit length . This is calculated by measuring the length of weld bead deposited per unit length of consumed electrode: Run-Out Ratio = Length of Weld Bead Produced (inches) Length of Electrode Consumed (inches) \text{Run-Out Ratio} = \frac{\text{Length of Weld Bead Produced (inches)}}{\text{Length of Electrode Consumed (inches)}} Run-Out Ratio = Length of Electrode Consumed (inches) Length of Weld Bead Produced (inches)
An increase in bead width (e.g., changing from a narrow stringer bead to a wide weave bead) increases the volume of weld metal per unit length, which increases local heat input and slows the cooling rate, degrading HAZ toughness.
Advanced Waveform Control Power Sources
Modern pulsed GMAW and computerized power sources modulate current and voltage thousands of times per second. Paragraph QW-409.1 explicitly addresses these power supplies by requiring the use of Instantaneous Energy ( J J J ) or Instantaneous Power ( W W W ) measured by specialized internal meters: Energy per Unit Length ( J / in. ) = Total Instantaneous Energy ( J ) Bead Length ( in. ) \text{Energy per Unit Length } (J/\text{in.}) = \frac{\text{Total Instantaneous Energy } (J)}{\text{Bead Length } (\text{in.})} Energy per Unit Length ( J / in. ) = Bead Length ( in. ) Total Instantaneous Energy ( J )
Conventional average meters ( V avg × A avg V_{\text{avg}} \times A_{\text{avg}} V avg × A avg ) are mathematically inaccurate for pulsed waveforms and cannot be used for code compliance when waveform-controlled machines are specified.
4. Postweld Heat Treatment (PWHT) Holding Time Limits: Paragraph QW-407.2
In non-toughness procedures under QW-407.1, PWHT is categorized broadly into six basic conditions (e.g., none, below lower transformation temperature, above upper transformation, etc.). However, when impact testing is required, time-at-temperature becomes critical.
The 80% Rule (QW-407.2)
Paragraph QW-407.2 mandates:
A change in postweld heat treatment temperature range requires requalification.
For test coupons subjected to PWHT below the lower transformation temperature, the total holding time at temperature recorded on the PQR must represent at least 80% of the total aggregate time to which the production material will be subjected during fabrication, intermediate heat treatments, and anticipated weld repairs. PQR PWHT Time ≥ 0.80 × Total Planned Production PWHT Time \text{PQR PWHT Time} \ge 0.80 \times \text{Total Planned Production PWHT Time} PQR PWHT Time ≥ 0.80 × Total Planned Production PWHT Time Maximum Qualified Production PWHT Time = PQR PWHT Time 0.80 = 1.25 × PQR PWHT Time \text{Maximum Qualified Production PWHT Time} = \frac{\text{PQR PWHT Time}}{0.80} = 1.25 \times \text{PQR PWHT Time} Maximum Qualified Production PWHT Time = 0.80 PQR PWHT Time = 1.25 × PQR PWHT Time
Metallurgical Rationale: Tempering and Carbide Coarsening
When welded steel is held at PWHT temperatures (typically 1100 ∘ F 1100^\circ\text{F} 110 0 ∘ F to 1350 ∘ F 1350^\circ\text{F} 135 0 ∘ F / 595 ∘ C 595^\circ\text{C} 59 5 ∘ C to 730 ∘ C 730^\circ\text{C} 73 0 ∘ C ) for extended periods, several metallurgical degradation mechanisms occur:
Dislocation Annihilation: The dislocation density decreases, softening the matrix and reducing yield and tensile strength.
Carbide Coarsening (Ostwald Ripening): Fine, finely dispersed iron and alloy carbides dissolve and reprecipitate as massive, coarse carbides along grain boundaries.
Intergranular Embrittlement: Massive grain boundary carbides act as severe stress raisers and cleavage initiation sites, drastically lowering absorbed Charpy energy.
If a PQR coupon is heat treated for only 1 hour, but production vessels undergo multiple PWHT cycles totaling 4 hours (initial PWHT, intermediate cycles, plus post-repair PWHT), the production weldment will suffer catastrophic toughness loss. The 80% rule guarantees that test coupons reflect the real thermal history of the finished component.
5. Construction Code Interfacing: ASME B31.1 vs. ASME B31.3 Toughness Rules
- Feature ASME B31.1 (Power Piping) ASME B31.3 (Process Piping)
- Governing Paragraphs Paragraph 107.8 & Table 107.8.2 Paragraph 323.2, 323.3 & Table 323.2.2
Toughness Exemption Rules Specific exemptions based on material spec and design temperature Exemption curves (Curves A, B, C, D in Fig. 323.2.2A) and Table 323.2.2
- Specimen Locations Weld metal center and HAZ Weld metal center and HAZ (fusion line + 1 mm)
- Specimen Count per Set 3 Weld Metal + 3 HAZ specimens 3 Weld Metal + 3 HAZ specimens per temperature
Acceptance Criteria Typically 15 ft-lbs (20 J) avg for carbon steels Based on material minimum yield strength and thickness (Table 323.3.5)
Lateral Expansion Required when specified by engineering Mandated for austenitic stainless steels and high-strength alloys
ASME B31.3 Specimen Location Rules
Under ASME B31.3 paragraph 323.3.4, when procedure qualification impact testing is required:
Weld Metal Specimens: Three Charpy V-notch specimens extracted transversely from the weld deposit, with the notch oriented perpendicular to the surface and located entirely within the weld centerline.
HAZ Specimens: Three Charpy V-notch specimens extracted transversely, with the notch located in the heat-affected zone such that the notch intersects the fusion line and HAZ microstructure as required by the code.
- 6. Worked Inspection Scenarios & Audit Calculations
- Scenario 1: Auditing an Impact-Tested WPS Thickness Range
A quality inspector reviews a WPS for an ASME B31.3 low-temperature ethylene piping system operating at − 50 ∘ F -50^\circ\text{F} − 5 0 ∘ F ( − 45 ∘ C -45^\circ\text{C} − 4 5 ∘ C ). The supporting PQR was welded on ASTM A333 Grade 6 seamless pipe with a nominal wall thickness of T = 0.500 in. T = 0.500\text{ in.} T = 0.500 in. ( 1 / 2 in. 1/2\text{ in.} 1/2 in. ). The PQR passed Charpy impact testing at − 50 ∘ F -50^\circ\text{F} − 5 0 ∘ F . The WPS lists the qualified base metal thickness range as 3 / 16 in. 3/16\text{ in.} 3/16 in. to 1.0 in. 1.0\text{ in.} 1.0 in.
Audit Evaluation: Nonconformance! The welding engineer incorrectly copied the non-toughness range from Table QW-451.1 ( 3 / 16 in. 3/16\text{ in.} 3/16 in. to 2 T 2T 2 T ). Because impact testing is required by ASME B31.3, paragraph QW-403.6 governs the minimum thickness. For T = 0.500 in. T = 0.500\text{ in.} T = 0.500 in. , T T T is between 1 / 4 in. 1/4\text{ in.} 1/4 in. and 5 / 8 in. 5/8\text{ in.} 5/8 in. , so the qualified minimum is equal to T T T ( 0.500 in. 0.500\text{ in.} 0.500 in. ). The legal WPS range is 0.500 in. 0.500\text{ in.} 0.500 in. to 1.000 in. 1.000\text{ in.} 1.000 in. The WPS cannot be used to weld pipe thinner than 0.500 in. 0.500\text{ in.} 0.500 in.
Scenario 2: Heat Input Verification on Shop Traveler
A piping fabricator welds an ASME B31.3 impact-tested joint using SMAW with E7018-1. The certified PQR documents the following parameters:
Voltage: 24 V, Amperage: 160 A, Travel Speed: 5.5 inches per minute (ipm).
PQR Qualified Heat Input: H PQR = 24 × 160 × 60 5.5 × 1000 = 230 , 400 5 , 500 = 41.89 kJ/in. H_{\text{PQR}} = \frac{24 \times 160 \times 60}{5.5 \times 1000} = \frac{230,400}{5,500} = 41.89\text{ kJ/in.} H PQR = 5.5 × 1000 24 × 160 × 60 = 5 , 500 230 , 400 = 41.89 kJ/in.
During a shop floor audit, the CWI observes a welder running a wide weave cap pass with the following monitored parameters: Voltage: 26 V, Amperage: 175 A, Travel Speed: 4.2 ipm.
Actual Production Heat Input: H actual = 26 × 175 × 60 4.2 × 1000 = 273 , 000 4 , 200 = 65.00 kJ/in. H_{\text{actual}} = \frac{26 \times 175 \times 60}{4.2 \times 1000} = \frac{273,000}{4,200} = 65.00\text{ kJ/in.} H actual = 4.2 × 1000 26 × 175 × 60 = 4 , 200 273 , 000 = 65.00 kJ/in.
Compliance Determination: Critical Violation of QW-409.1. The production heat input ( 65.00 kJ/in. 65.00\text{ kJ/in.} 65.00 kJ/in. ) exceeds the qualified maximum ( 41.89 kJ/in. 41.89\text{ kJ/in.} 41.89 kJ/in. ) by 55%. The excessive heat input slows the cooling rate, promoting grain coarsening and severe embrittlement. The weld must be rejected and the joint cut out or requalified.
Scenario 3: PWHT Aggregate Time Verification
A pressure vessel component requires 2 hours of postweld heat treatment during initial shop fabrication, and the engineering specification anticipates a potential 1.5-hour post-repair PWHT cycle during vessel installation, for a total planned aggregate PWHT time of 3.5 hours 3.5\text{ hours} 3.5 hours . What is the minimum PWHT soak time that must be applied to the PQR qualification test coupon?
Calculation under QW-407.2: Minimum PQR Time = 0.80 × 3.5 hours = 2.80 hours = 2 hours, 48 minutes \text{Minimum PQR Time} = 0.80 \times 3.5\text{ hours} = 2.80\text{ hours} = 2\text{ hours, } 48\text{ minutes} Minimum PQR Time = 0.80 × 3.5 hours = 2.80 hours = 2 hours, 48 minutes
If the PQR coupon was heat treated for only 2.0 hours, it qualifies a maximum production PWHT time of 2.0 / 0.80 = 2.5 hours 2.0 / 0.80 = 2.5\text{ hours} 2.0/0.80 = 2.5 hours , which is insufficient to cover the required 3.5-hour aggregate envelope.