Study guide

2.2 Mechanical Test Types, Specimen Dimensions & Acceptance Criteria

AWS ASME BPVC Section IX + B31.1/B31.3 Endorsement CWI/SCWI

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: Exam Structure, Logistics & Code Navigation Strategy

1.1 Credential Overview, Prometric Delivery & July 2025 Hard-Copy Rule 1.2 The Three-Code Triad: Section IX, B31.1, and B31.3 Roles & Interrelationships 1.3 Rapid Code-Book Navigation: Tabbing, Cross-Referencing & Time Management

2 Chapter 2: Section IX Article I — General Welding Requirements

2.1 Scope, Responsibilities & Section IX Architecture 2.2 Mechanical Test Types, Specimen Dimensions & Acceptance Criteria 2.3 Notch-Toughness Tests, Fillet-Weld Tests & Special Examinations

3 Chapter 3: Section IX Article II — Procedure Qualification Fundamentals

3.1 PQR vs. WPS Workflow, Purpose & Content Requirements 3.2 Coupling and Supporting Multiple WPSs and PQRs 3.3 Test Coupons, Preparation & Required Test Specimen Allocations

4 Chapter 4: Section IX Procedure Qualification Limits & Thickness Rules

4.1 Base Metal & Deposited Weld Metal Thickness Limits 4.2 Impact Testing Requirements & Toughness Thickness Qualification Ranges 4.3 Fillet Weld Procedure Qualification Rules & Special Applications

5 Chapter 5: Section IX Article III — Welder Performance Qualification Fundamentals

5.1 Welder & Welding Operator Qualification Intent, Responsibilities & Identification 5.2 Qualification Testing Methods: Mechanical Bend Tests vs. Volumetric NDE 5.3 Welder Qualification Continuity, Expiration, and Requalification

6 Chapter 6: Section IX Welder Performance Limits, Positions & Diameters

6.1 Test Positions, Groove Weld Orientations & Production Position Limits 6.2 Welder Thickness Limits and Pipe Diameter Qualification Ranges 6.3 Welder Essential Variables: F-Numbers, Backing, and Process Transfers

7 Chapter 7: Section IX Article IV — Welding Variables by Process (Part 1: SMAW & GTAW)

7.1 Understanding Essential, Supplementary Essential & Nonessential Variables 7.2 Shielded Metal Arc Welding (SMAW) Procedure Variables 7.3 Gas Tungsten Arc Welding (GTAW) Procedure Variables

8 Chapter 8: Section IX Article IV — Welding Variables by Process (Part 2: GMAW/FCAW & SAW)

8.1 GMAW & FCAW Procedure Variables and Short-Circuiting Transfer Rules 8.2 Submerged Arc Welding (SAW) Procedure Variables and Flux-Wire Combinations 8.3 Special Variables: Heat Input, Electrical Characteristics & Shielding Gases

9 Chapter 9: Section IX Material Classifications, Numbers & Standard Documentation

9.1 Base Metal P-Numbers, Group Numbers, and S-Numbers 9.2 Filler Metal F-Numbers and As-Deposited Chemistry A-Numbers 9.3 ASME Standard Documentation: Auditing WPS, PQR, and WPQ Forms

10 Chapter 10: ASME B31.1 Power Piping — Scope, Materials, Design & Welding Fabrication

10.1 B31.1 Scope, Jurisdiction, Boiler External Piping vs. Non-Boiler External Piping 10.2 B31.1 Welding Requirements, Joint Alignment, Backing Rings & Tack Welds 10.3 B31.1 Welder & Procedure Qualification Interfacing with Section IX 10.4 B31.1 Materials, Design Conditions & Pressure Design of Components

11 Chapter 11: ASME B31.1 Power Piping — Heat Treatment, Examination, Testing & Fabrication Records

11.1 B31.1 Preheat Rules & Mandatory Temperatures 11.2 B31.1 Postweld Heat Treatment (PWHT) Rules, Temperatures & Holding Times 11.3 B31.1 Mandatory NDE Examination, Acceptance Standards & Pressure Leak Tests 11.4 B31.1 Bending, Forming, Assembly & Code Records

12 Chapter 12: ASME B31.3 Process Piping — Scope, Fluid Services, Materials, Design & Welding

12.1 B31.3 Scope, Fluid Service Classifications & Owner Responsibilities 12.2 B31.3 Welding, Joint Preparation, Backing Rings & Fabrication Details 12.3 B31.3 Procedure & Performance Qualification Rules and Section IX Exceptions 12.4 B31.3 Materials, Design Conditions & Pressure Design of Components

13 Chapter 13: ASME B31.3 Process Piping — Heat Treatment, Examination, Testing, Fabrication & Records

13.1 B31.3 Preheat and Postweld Heat Treatment Rules & Tables 13.2 B31.3 Inspection vs. Examination Responsibilities & Examination Extents 13.3 B31.3 Acceptance Criteria for Weld Imperfections 13.4 B31.3 Pressure Leak Testing: Hydrostatic, Pneumatic & Sensitive Leak Tests 13.5 B31.3 Bending, Forming, Assembly & Records

2.2 Mechanical Test Types, Specimen Dimensions & Acceptance Criteria

Key Takeaways Explain This Topic AI

Tension testing (QW-150) measures the ultimate tensile strength of the procedure qualification weldment; test specimens must be prepared in accordance with QW-462.1 with weld reinforcement removed flush.

Under QW-153.1, if a tension specimen breaks in the weld metal, it must meet or exceed the Minimum Specified Tensile Strength (MSTS) of the base metal; if it breaks in the base metal outside the weld or fusion line, it passes if the strength is not less than 95% of the MSTS.

When joining dissimilar base metals of different tensile strengths, the minimum required tensile strength for procedure acceptance is governed by the weaker base metal (or 95% of the weaker base metal if failure occurs in that base metal outside the fusion line).

Guided-bend testing (QW-160) evaluates soundness and ductility; transverse side bends (QW-161.1) are standard for thickness T ≥ 3/4 in. (19 mm), whereas transverse face/root bends (QW-161.2/161.3) are standard for thin materials.

Under QW-163, guided-bend specimens are acceptable if no open discontinuity in the weld or HAZ exceeds 1/8 in. (3 mm) in any direction; open corner cracks ≤ 1/4 in. (6 mm) are ignored unless caused by slag inclusions, lack of fusion, or internal defects.

Last updated: September 2026

2.2 Mechanical Test Types, Specimen Dimensions & Acceptance Criteria

In ASME Section IX Article I, mechanical testing constitutes the definitive barrier between an unproven welding concept and a qualified, code-compliant fabrication procedure. When qualifying a groove welding procedure, Section IX relies on two primary destructive test types:

Tension Tests (QW-150) : Designed to measure the ultimate tensile capacity and load-bearing efficiency of the weldment relative to the base metal.

Guided-Bend Tests (QW-160) : Designed to assess the ductility, soundness, and fusion integrity of both the weld metal and the heat-affected zone (HAZ).

Inspectors taking the AWS Endorsement examination must be fluent in specimen geometry, dimensional tolerances, mathematical formulas, and the precise pass/fail criteria stipulated by paragraphs QW-153 and QW-163.

1. Tension Tests (QW-150)

Tension test specimens are machined from the welded procedure test coupon after all required non-destructive examinations (and postweld heat treatments, if applicable) are completed. Section IX requires a minimum of two tension test specimens for standard groove weld procedure qualification (QW-451.1).

Specimen Preparation & Geometry (QW-151 & QW-462.1)

Tension specimens may take several standardized forms depending on material thickness, form (plate vs. pipe), and testing machine capacity:

Reduced Section — Plate (QW-462.1(a)) :

Standard specimen width: 0.750 in. 0.750\text{ in.} 0.750 in. (19 mm) for thickness T ≤ 1 in. T \le 1\text{ in.} T ≤ 1 in. , or 1.50 in. 1.50\text{ in.} 1.50 in. (38 mm) for thin sheet/plate.

Parallel reduced section length: The weld width plus at least 0.50 in. 0.50\text{ in.} 0.50 in. (13 mm) on each side, with a minimum parallel length of 2.25 in. 2.25\text{ in.} 2.25 in. (57 mm).

Transition radius: Minimum 1.0 in. 1.0\text{ in.} 1.0 in. (25 mm) radius to prevent stress concentrations at the grips.

Weld reinforcement removal: Under QW-151.1, the weld reinforcement must be machined or ground flush with the surfaces of the base metal.

Reduced Section — Pipe (QW-462.1(b)) :

Used for pipe diameters ≥ 3 in. \ge 3\text{ in.} ≥ 3 in. OD. Longitudinal strip specimens machined with parallel sides and weld reinforcement removed flush.

Turned (Round) Specimens (QW-462.1(c)) :

For thick materials ( T > 1 in. T > 1\text{ in.} T > 1 in. [25 mm]), round turned specimens with gage diameters of 0.505 in. 0.505\text{ in.} 0.505 in. , 0.353 in. 0.353\text{ in.} 0.353 in. , or 0.252 in. 0.252\text{ in.} 0.252 in. may be extracted. Alternatively, full-thickness slabs can be sliced into multiple longitudinal rectangular slices (multi-specimen sets).

Full-Section Pipe (QW-462.1(d)) :

Used for small diameter pipe (nominal OD ≤ 3 in. \le 3\text{ in.} ≤ 3 in. ). Snug-fitting metal plugs are inserted into the pipe ends to prevent collapse inside the testing machine grips.

Tensile Strength Calculation

The ultimate tensile strength ( R m R_m R m ​ or UTS) is calculated by dividing the maximum ultimate load ( P P P ) sustained by the specimen prior to rupture by the original cross-sectional area ( A A A ) of the reduced section: Tensile Strength (psi or MPa) = Ultimate Breaking Load ( P ) Original Cross-Sectional Area ( A ) \text{Tensile Strength (psi or MPa)} = \frac{\text{Ultimate Breaking Load } (P)}{\text{Original Cross-Sectional Area } (A)} Tensile Strength (psi or MPa) = Original Cross-Sectional Area ( A ) Ultimate Breaking Load ( P ) ​

Where cross-sectional area for rectangular specimens is: A = Width ( w ) × Thickness ( t ) A = \text{Width } (w) \times \text{Thickness } (t) A = Width ( w ) × Thickness ( t )

Note for Inspectors : All cross-sectional dimensions must be measured with calibrated precision micrometers prior to pulling the specimen.

Tensile Acceptance Criteria (QW-153.1)

Paragraph QW-153.1 dictates the four distinct conditions under which a tension specimen is accepted: [Tension Specimen Ruptures]

  • │
  • ┌──────────────────────┴──────────────────────┐
  • ▼ ▼
  • [Break in Weld Metal] [Break in Base Metal]
  • │ │
  • ▼ ▼
  • Tensile Strength MUST be Did break occur outside the

>= Minimum Specified weld and fusion line?

  • Tensile Strength (MSTS) │
  • of Base Metal! ├───────────────┐
  • (No 95% reduction allowed!) ▼ ▼
  • [YES] [NO]
  • │ (At Fusion Line)
  • ▼ │
  • Tensile Strength ▼
  • MUST be >= 95% Treated as weld
  • of Base Metal break: MUST be

MSTS! >= MSTS!

Failure in Weld Metal (QW-153.1(a)) : If the specimen ruptures in the weld metal, the calculated tensile strength shall not be less than the Minimum Specified Tensile Strength (MSTS) of the base metal as listed in Section IX Table QW/QB-422.

Failure in Base Metal Outside Weld/Fusion Line (QW-153.1(b)) : If the specimen ruptures in the base metal outside of the weld and weld interface (fusion line), the test is acceptable provided the tensile strength is not more than 5% below the MSTS of the base metal (i.e., at least 95% of MSTS ).

Metallurgical Rationale : Heat from welding can produce localized annealing in cold-worked or heat-treated base metals, slightly softening the HAZ or adjacent parent metal. Section IX tolerates up to a 5% drop in base metal strength as an inherent artifact of thermal welding cycles.

Dissimilar Base Metal Welds (QW-153.1(c)) : If two base metals of different MSTS are joined, the tensile strength shall not be less than the MSTS of the weaker base metal . If the rupture occurs in the weaker base metal outside the fusion line, the strength shall not be less than 95% of the MSTS of that weaker base metal .

Base Metals Without Specified Tensile Strength (QW-153.1(d)) : For materials not listed in QW/QB-422, acceptance is governed by the referencing construction code.

2. Guided-Bend Tests (QW-160)

While tension tests establish load capacity, guided-bend tests verify that the weld metal and HAZ can undergo severe plastic deformation without initiating or propagating planar defects.

Specimen Types & Orientations (QW-161)

Bend specimens are categorized based on the surface that is stretched into convex tension:

Transverse Side Bend (QW-161.1) : The specimen is cut transverse to the longitudinal axis of the weld and bent so that one of the side cut surfaces becomes the convex (stretched) surface. Standard side bend thickness is t = 3 / 8 in. t = 3/8\text{ in.} t = 3/8 in. ( 10 mm 10\text{ mm} 10 mm ). Side bends evaluate the entire through-thickness of the weldment from face to root simultaneously.

Transverse Face Bend (QW-161.2) : The specimen is cut transverse to the weld axis and bent so that the original weld face becomes the convex outer surface.

Transverse Root Bend (QW-161.3) : The specimen is cut transverse to the weld axis and bent so that the original weld root becomes the convex outer surface.

Longitudinal Face Bend (QW-161.4) & Longitudinal Root Bend (QW-161.5) : The specimen is cut parallel to the weld axis. Used primarily when joining base metals or depositing filler metals that have substantially different mechanical properties (e.g., austenitic stainless steel welded to ferritic carbon steel, or high-nickel alloys), where transverse bending would cause uneven straining across the joint.

Thickness Selection Rules (QW-451.1)

Coupon Thickness T < 3 / 8 in. T < 3/8\text{ in.} T < 3/8 in. (10 mm) : Transverse Face and Root bends are standard.

Coupon Thickness 3 / 8 in. ≤ T < 3 / 4 in. 3/8\text{ in.} \le T < 3/4\text{ in.} 3/8 in. ≤ T < 3/4 in. (10 mm to 19 mm) : Either 4 side bends OR 2 face bends and 2 root bends are permitted.

Coupon Thickness T ≥ 3 / 4 in. T \ge 3/4\text{ in.} T ≥ 3/4 in. (19 mm) : Side bends are mandatory (4 side bend specimens required). Face and root bends are not permitted for thick coupons because outer fiber strain cannot effectively interrogate the core of the weldment.

Bend Test Jigs (QW-162 & QW-466)

Section IX specifies three distinct jig configurations in Article IV:

Standard Guided-Bend Jig (QW-466.1) : Uses a hydraulic or mechanical plunger forcing the specimen into a contoured die. For standard P-No. 1 carbon steels with t = 3 / 8 in. t = 3/8\text{ in.} t = 3/8 in. , the plunger radius is A / 2 = 0.75 in. A/2 = 0.75\text{ in.} A /2 = 0.75 in. ( A = 1.50 in. = 4 t A = 1.50\text{ in.} = 4t A = 1.50 in. = 4 t ), and die width is B = 2.0625 in. B = 2.0625\text{ in.} B = 2.0625 in. ( 2 − 1 / 16 in. 2-1/16\text{ in.} 2 − 1/16 in. ). This imposes approximately 20% outer fiber elongation.

Guided-Bend Roller Jig (QW-466.2) : Replaces fixed die shoulders with hardened rotating rollers to reduce sliding friction and prevent galling.

Wrap-Around Guided-Bend Jig (QW-466.3) : Clamps one end of the specimen securely against a central mandrel while a roller wraps the specimen around the pin. This eliminates compressive buckling and is strongly favored for thin sheets and work-hardening materials.

Guided-Bend Acceptance Criteria (QW-163)

Paragraph QW-163 provides clear, quantitative rejection thresholds. After bending through a full 180 ∘ 180^\circ 18 0 ∘ arc:

The weld metal and HAZ must be completely within the bent portion of the specimen.

Discontinuity Limit : There shall be no open discontinuity exceeding 1/8 in. (3 mm) measured in any direction on the convex surface of the specimen in the weld metal or HAZ.

Corner Crack Exception : Cracks occurring on the corners of the specimen during bending shall not be considered , provided they do not exceed 1/4 in. (6 mm) and there is no metallurgical evidence that they resulted from lack of fusion, slag inclusions, or other internal weld defects.

If a corner crack exhibits slag, lack of penetration, or porosity, it is treated as an internal defect and must not exceed the strict 1/8 in. (3 mm) limit.

Corrosion-Resistant Overlay Cladding : Open defects in the cladding layer must not exceed 1 / 16 in. 1/16\text{ in.} 1/16 in. ( 1.5 mm 1.5\text{ mm} 1.5 mm ), and open defects at the bond line must not exceed 1 / 8 in. 1/8\text{ in.} 1/8 in. ( 3 mm 3\text{ mm} 3 mm ).

  • 3. Practical Calculation & Evaluation Scenarios
  • Case Study 1: Tensile Evaluation on SA-516 Grade 70

A PQR test coupon welded from 0.500 in. 0.500\text{ in.} 0.500 in. thick SA-516 Grade 70 plate is tested. From ASME Section IX Table QW/QB-422, the Minimum Specified Tensile Strength (MSTS) for SA-516 Gr 70 is 70,000 psi .

Two reduced-section specimens are pulled:

Specimen T-1 :

Measured dimensions: Width w = 0.752 in. w = 0.752\text{ in.} w = 0.752 in. , Thickness t = 0.495 in. t = 0.495\text{ in.} t = 0.495 in.

Area A = 0.752 × 0.495 = 0.37224 sq in. A = 0.752 \times 0.495 = 0.37224\text{ sq in.} A = 0.752 × 0.495 = 0.37224 sq in.

  • Ultimate Load P = 25 , 900 lbf P = 25,900\text{ lbf} P = 25 , 900 lbf
  • Failure location: Weld metal

Calculated UTS: 25 , 900 / 0.37224 = 69 , 579 psi 25,900 / 0.37224 = 69,579\text{ psi} 25 , 900/0.37224 = 69 , 579 psi

Evaluation : FAIL . The specimen ruptured in the weld metal at 69 , 579 psi 69,579\text{ psi} 69 , 579 psi , which is below the mandatory MSTS of 70 , 000 psi 70,000\text{ psi} 70 , 000 psi . Under QW-153.1(a), weld breaks receive no tolerance.

Specimen T-2 :

Measured dimensions: Width w = 0.750 in. w = 0.750\text{ in.} w = 0.750 in. , Thickness t = 0.498 in. t = 0.498\text{ in.} t = 0.498 in.

Area A = 0.750 × 0.498 = 0.37350 sq in. A = 0.750 \times 0.498 = 0.37350\text{ sq in.} A = 0.750 × 0.498 = 0.37350 sq in.

  • Ultimate Load P = 25 , 200 lbf P = 25,200\text{ lbf} P = 25 , 200 lbf
  • Failure location: Base metal, 1.25 inches outside the fusion line

Calculated UTS: 25 , 200 / 0.37350 = 67 , 470 psi 25,200 / 0.37350 = 67,470\text{ psi} 25 , 200/0.37350 = 67 , 470 psi

Minimum required for base metal failure: 0.95 × 70 , 000 psi = 66 , 500 psi 0.95 \times 70,000\text{ psi} = 66,500\text{ psi} 0.95 × 70 , 000 psi = 66 , 500 psi

Evaluation : PASS . The specimen ruptured in the base metal outside the weld at 67 , 470 psi 67,470\text{ psi} 67 , 470 psi , which exceeds the 95% threshold of 66 , 500 psi 66,500\text{ psi} 66 , 500 psi per QW-153.1(b).

Case Study 2: Side Bend Evaluation with Discontinuities

A CWI inspects four side bend specimens tested in a guided-bend jig:

Specimen B-1 : Displays an opening in the center of the weld metal measuring 0.100 in. 0.100\text{ in.} 0.100 in. long by 0.040 in. 0.040\text{ in.} 0.040 in. wide. ( 0.100 in. < 1 / 8 in. 0.100\text{ in.} < 1/8\text{ in.} 0.100 in. < 1/8 in. [0.125 in.]). -> ACCEPTABLE .

Specimen B-2 : Displays an opening along the fusion line measuring 0.140 in. 0.140\text{ in.} 0.140 in. in length. ( 0.140 in. > 1 / 8 in. 0.140\text{ in.} > 1/8\text{ in.} 0.140 in. > 1/8 in. ). -> REJECT .

Specimen B-3 : Displays a tear on the sharp corner of the specimen measuring 0.1875 in. 0.1875\text{ in.} 0.1875 in. ( 3 / 16 in. 3/16\text{ in.} 3/16 in. ) long. Visual examination shows cleanly torn parent grain structure with no slag, inclusions, or unbonded sidewall. -> ACCEPTABLE (corner crack ≤ 1 / 4 in. \le 1/4\text{ in.} ≤ 1/4 in. without underlying weld defects per QW-163).

Specimen B-4 : Displays a corner tear measuring 0.150 in. 0.150\text{ in.} 0.150 in. ( < 1 / 4 in. < 1/4\text{ in.} < 1/4 in. ), but optical magnification reveals trapped black slag particles in the root of the tear. -> REJECT (because slag is present, the 1 / 8 in. 1/8\text{ in.} 1/8 in. [0.125 in.] threshold applies, and 0.150 in. > 0.125 in. 0.150\text{ in.} > 0.125\text{ in.} 0.150 in. > 0.125 in. ).

Loading diagram... Decision Tree for Acceptance of Section IX Tension and Guided-Bend Specimens