8.1 GMAW & FCAW Procedure Variables and Short-Circuiting Transfer Rules
AWS ASME BPVC Section IX + B31.1/B31.3 Endorsement CWI/SCWI
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Exam Structure, Logistics & Code Navigation Strategy
1.1 Credential Overview, Prometric Delivery & July 2025 Hard-Copy Rule 1.2 The Three-Code Triad: Section IX, B31.1, and B31.3 Roles & Interrelationships 1.3 Rapid Code-Book Navigation: Tabbing, Cross-Referencing & Time Management
2 Chapter 2: Section IX Article I — General Welding Requirements
2.1 Scope, Responsibilities & Section IX Architecture 2.2 Mechanical Test Types, Specimen Dimensions & Acceptance Criteria 2.3 Notch-Toughness Tests, Fillet-Weld Tests & Special Examinations
3 Chapter 3: Section IX Article II — Procedure Qualification Fundamentals
3.1 PQR vs. WPS Workflow, Purpose & Content Requirements 3.2 Coupling and Supporting Multiple WPSs and PQRs 3.3 Test Coupons, Preparation & Required Test Specimen Allocations
4 Chapter 4: Section IX Procedure Qualification Limits & Thickness Rules
4.1 Base Metal & Deposited Weld Metal Thickness Limits 4.2 Impact Testing Requirements & Toughness Thickness Qualification Ranges 4.3 Fillet Weld Procedure Qualification Rules & Special Applications
5 Chapter 5: Section IX Article III — Welder Performance Qualification Fundamentals
5.1 Welder & Welding Operator Qualification Intent, Responsibilities & Identification 5.2 Qualification Testing Methods: Mechanical Bend Tests vs. Volumetric NDE 5.3 Welder Qualification Continuity, Expiration, and Requalification
6 Chapter 6: Section IX Welder Performance Limits, Positions & Diameters
6.1 Test Positions, Groove Weld Orientations & Production Position Limits 6.2 Welder Thickness Limits and Pipe Diameter Qualification Ranges 6.3 Welder Essential Variables: F-Numbers, Backing, and Process Transfers
7 Chapter 7: Section IX Article IV — Welding Variables by Process (Part 1: SMAW & GTAW)
7.1 Understanding Essential, Supplementary Essential & Nonessential Variables 7.2 Shielded Metal Arc Welding (SMAW) Procedure Variables 7.3 Gas Tungsten Arc Welding (GTAW) Procedure Variables
8 Chapter 8: Section IX Article IV — Welding Variables by Process (Part 2: GMAW/FCAW & SAW)
8.1 GMAW & FCAW Procedure Variables and Short-Circuiting Transfer Rules 8.2 Submerged Arc Welding (SAW) Procedure Variables and Flux-Wire Combinations 8.3 Special Variables: Heat Input, Electrical Characteristics & Shielding Gases
9 Chapter 9: Section IX Material Classifications, Numbers & Standard Documentation
9.1 Base Metal P-Numbers, Group Numbers, and S-Numbers 9.2 Filler Metal F-Numbers and As-Deposited Chemistry A-Numbers 9.3 ASME Standard Documentation: Auditing WPS, PQR, and WPQ Forms
10 Chapter 10: ASME B31.1 Power Piping — Scope, Materials, Design & Welding Fabrication
10.1 B31.1 Scope, Jurisdiction, Boiler External Piping vs. Non-Boiler External Piping 10.2 B31.1 Welding Requirements, Joint Alignment, Backing Rings & Tack Welds 10.3 B31.1 Welder & Procedure Qualification Interfacing with Section IX 10.4 B31.1 Materials, Design Conditions & Pressure Design of Components
11 Chapter 11: ASME B31.1 Power Piping — Heat Treatment, Examination, Testing & Fabrication Records
11.1 B31.1 Preheat Rules & Mandatory Temperatures 11.2 B31.1 Postweld Heat Treatment (PWHT) Rules, Temperatures & Holding Times 11.3 B31.1 Mandatory NDE Examination, Acceptance Standards & Pressure Leak Tests 11.4 B31.1 Bending, Forming, Assembly & Code Records
12 Chapter 12: ASME B31.3 Process Piping — Scope, Fluid Services, Materials, Design & Welding
12.1 B31.3 Scope, Fluid Service Classifications & Owner Responsibilities 12.2 B31.3 Welding, Joint Preparation, Backing Rings & Fabrication Details 12.3 B31.3 Procedure & Performance Qualification Rules and Section IX Exceptions 12.4 B31.3 Materials, Design Conditions & Pressure Design of Components
13 Chapter 13: ASME B31.3 Process Piping — Heat Treatment, Examination, Testing, Fabrication & Records
13.1 B31.3 Preheat and Postweld Heat Treatment Rules & Tables 13.2 B31.3 Inspection vs. Examination Responsibilities & Examination Extents 13.3 B31.3 Acceptance Criteria for Weld Imperfections 13.4 B31.3 Pressure Leak Testing: Hydrostatic, Pneumatic & Sensitive Leak Tests 13.5 B31.3 Bending, Forming, Assembly & Records
8.1 GMAW & FCAW Procedure Variables and Short-Circuiting Transfer Rules
Key Takeaways Explain This Topic AI
Under Table QW-255, a change from globular, spray, or pulsed spray transfer to the short-circuiting transfer mode (GMAW-S), or vice versa, is an essential variable per QW-409.2 mandating complete procedure requalification.
Short-circuiting GMAW triggers two separate essential variables: QW-403.10 caps the qualified base metal thickness at 1.1T when the coupon thickness T is under 1/2 in. (13 mm), and QW-404.32 caps the qualified deposited weld metal at 1.1t when the deposit t is under 1/2 in. (13 mm).
Under QW-404.23, changing between solid wire (GMAW), metal-cored wire (MCAW), and flux-cored wire (FCAW) is an essential variable requiring a new PQR, even if the filler metals share the same AWS F-number (F-No. 6).
A change from a single shielding gas to any other gas, or a change in nominal composition of a gas mixture of greater than 5%, is an essential variable under QW-408.2.
Flux-Cored Arc Welding (FCAW) is governed entirely by Table QW-255 in ASME Section IX, sharing variable classifications with GMAW while introducing unique flux-core metallurgy and polarity considerations.
Last updated: September 2026
8.1 GMAW & FCAW Procedure Variables and Short-Circuiting Transfer Rules
Core Principle: In ASME Section IX, Gas Metal Arc Welding (GMAW) and Flux-Cored Arc Welding (FCAW) are co-located under Table QW-255. While both utilize a continuously fed consumable wire electrode, their arc physics, transfer mechanisms, and operational risks diverge sharply. The code enforces rigorous essential variable boundaries around metal transfer mode (QW-409.2), electrode product form (QW-404.23), shielding gas chemistry (QW-408.2), and low-thickness short-circuiting qualification limits (QW-403.10 and QW-404.32) to prevent catastrophic cold-lap and lack-of-fusion defects in production weldments.
1. Table QW-255 Architecture and Process Consolidation
Unlike structural codes (such as AWS D1.1) that treat GMAW and FCAW as separate welding processes with independent prequalification and qualification tables, ASME Section IX consolidates GMAW and FCAW into a single variable matrix: Table QW-255 .
This consolidation reflects their shared mechanical feed mechanisms, but Section IX embeds specific filler metal, electrical, and gas variables to account for their distinct metallurgical characteristics:
GMAW (Solid Wire): Relies on an external shielding gas to protect a solid, bare, or copper-coated continuous wire electrode. Slag formation is minimal (silicate islands).
MCAW (Metal-Cored Arc Welding): Uses a tubular wire filled with metallic powders (iron, ferro-alloys, deoxidizers). In Section IX, MCAW is categorized as GMAW (solid/bare wire classification), but governed by strict product form rules.
FCAW (Flux-Cored Arc Welding): Employs a tubular consumable wire containing non-metallic fluxing ingredients, mineral deoxidizers, and arc stabilizers. It may be gas-shielded (FCAW-G, dual shield) or self-shielded (FCAW-S). FCAW produces a continuous covering of protective slag over the solidified weld bead. +----------------------------------------------------------------------------------------------------+
- | TABLE QW-255 CONSOLIDATION ARCHITECTURE |
- +----------------------------------------------------------------------------------------------------+
- | PROCESS DESIGNATION | CONSUMABLE WIRE TYPE | SHIELDING MEDIUM | GOVERNING TABLE|
- +-----------------------------------+--------------------------+--------------------+----------------+
- | GMAW - Solid Wire | Solid bare wire | External Gas | Table QW-255 |
- | GMAW - Metal-Cored (MCAW) | Metal powder-cored tube | External Gas | Table QW-255 |
- | FCAW - Gas-Shielded (FCAW-G) | Flux/mineral-cored tube | External Gas | Table QW-255 |
- | FCAW - Self-Shielded (FCAW-S) | Gas-generating flux core | None (Flux vapor) | Table QW-255 |
- +----------------------------------------------------------------------------------------------------+
- 2. Table QW-255 Variable Classification Matrix
Welding engineers and CWI endorsement candidates must master the precise categorization of Table QW-255 variables into Essential , Supplementary Essential (toughness-dependent), and Nonessential .
- Variable Category Paragraph Variable Description Variable Status
- Joints (QW-402) QW-402.1 Deletion of backing Nonessential
- QW-402.4 Change in cross-section / groove design Nonessential
- QW-402.10 Change in root spacing Nonessential
- QW-402.11 Addition or deletion of retainers Nonessential
Base Metals (QW-403) QW-403.5 Change in base metal Group Number (when toughness applies) Supplementary Essential
- QW-403.6 Minimum base metal thickness T T T qualified (toughness) Supplementary Essential
- QW-403.8 Change in base metal thickness T T T qualified per QW-451 Essential
QW-403.9 Single-pass weld deposit t > 1 / 2 in. t > 1/2\text{ in.} t > 1/2 in. ( 13 mm 13\text{ mm} 13 mm ) Essential
- QW-403.10 Base metal thickness T T T limits for GMAW-S Essential
- Filler Metals (QW-404) QW-404.4 Change in F-Number Essential
- QW-404.5 Change in A-Number Essential
- QW-404.12 Change in AWS classification Nonessential
- QW-404.23 Change in product form (solid vs cored vs flux-cored) Essential
- QW-404.30 Change in deposited weld metal thickness t t t per QW-451 Essential
QW-404.32 GMAW-S deposit t < 1 / 2 in. t < 1/2\text{ in.} t < 1/2 in. restricts t max t_{\text{max}} t max to 1.1 t 1.1t 1.1 t Essential
- QW-404.33 Change in AWS classification when toughness applies Supplementary Essential
- Positions (QW-405) QW-405.1 Addition of one or more welding positions Nonessential
- QW-405.2 Change from any position to vertical-up Supplementary Essential
- QW-405.3 Change in vertical progression (vertical-up vs vertical-down) Nonessential
Preheat (QW-406) QW-406.1 Decrease of > 100 ∘ F > 100^\circ\text{F} > 10 0 ∘ F ( 55 ∘ C 55^\circ\text{C} 5 5 ∘ C ) in qualified preheat Essential
QW-406.3 Increase of > 100 ∘ F > 100^\circ\text{F} > 10 0 ∘ F ( 55 ∘ C 55^\circ\text{C} 5 5 ∘ C ) in interpass temp Supplementary Essential
PWHT (QW-407) QW-407.1 Change in PWHT condition (none, below A 1 A_1 A 1 , above A 3 A_3 A 3 , etc.) Essential
- QW-407.2 Change in PWHT time and temperature cycle Supplementary Essential
- Shielding Gas (QW-408) QW-408.1 Addition or deletion of shielding gas Essential
- QW-408.2 Change in single gas or nominal blend > 5 % > 5\% > 5% Essential
- QW-408.3 Change in shielding gas flow rate > 25 % > 25\% > 25% Nonessential
- QW-408.5 Addition or deletion of backing gas Essential
- QW-408.8 Deletion of backing gas Essential
Electrical (QW-409) QW-409.1 Increase in heat input or volume of weld metal per unit length Supplementary Essential
- QW-409.2 Change in transfer mode (GMAW-S vs globular/spray/pulsed) Essential
- QW-409.4 Change in current type (AC/DC) or polarity (DCEP/DCEN) Essential
- QW-409.8 Change in amperage, voltage, or wire feed speed range Nonessential
- Technique (QW-410) QW-410.1 Change from string to weave bead Nonessential
- QW-410.3 Change in shielding gas cup/nozzle orifice size Nonessential
- QW-410.9 Change from single to multiple electrodes (or vice versa) Essential
- QW-410.10 Change from single to multi-pass per side Supplementary Essential
- 3. Metal Transfer Modes and the QW-409.2 Mandate
In GMAW, the mode of metal transfer describes the physical mechanism by which molten droplets detach from the consumable electrode and enter the weld puddle. Operating conditions (shielding gas composition, arc voltage, welding current, and power source waveform) dictate the active transfer mode:
The Four Primary Metal Transfer Modes
Short-Circuiting Transfer (GMAW-S / Dip Transfer):
Operating Parameters: Low arc voltage ( 14 to 22 V 14\text{ to } 22\text{ V} 14 to 22 V ), low current ( 50 to 200 A 50\text{ to } 200\text{ A} 50 to 200 A ), small diameter wires ( 0.030 to 0.045 in. 0.030\text{ to } 0.045\text{ in.} 0.030 to 0.045 in. ). Suitable with 100 % CO 2 100\%\text{ CO}_2 100% CO 2 or 75 % Ar / 25 % CO 2 75\%\text{ Ar} / 25\%\text{ CO}_2 75% Ar /25% CO 2 .
Physics: The electrode wire contacts the weld pool directly at a rate of 20 to 200 times per second. During each physical short circuit, arc current surges, pinch force pinches off the droplet, and the arc re-ignites. Heat input is minimal.
Primary Risk: Lack of sidewall fusion ("cold lap") . On thick base materials ( T ≥ 1 / 2 in. T \ge 1/2\text{ in.} T ≥ 1/2 in. ), the low thermal energy fails to overcome the heatsinking capacity of the base metal, freezing molten filler metal against un-melted joint bevels.
Globular Transfer:
Operating Parameters: Intermediate arc voltage ( 22 to 28 V 22\text{ to } 28\text{ V} 22 to 28 V ), current exceeding short-circuit range but under the spray transition threshold. Typical in carbon steel welded with 100 % CO 2 100\%\text{ CO}_2 100% CO 2 or high CO 2 \text{CO}_2 CO 2 mixtures.
Physics: Droplets grow to diameters two to three times larger than the wire before detaching under gravity. Transfer is turbulent, erratic, and causes excessive spatter. Restricted to flat and horizontal fillet positions.
Axial Spray Transfer:
Operating Parameters: High arc voltage ( 26 to 35 V 26\text{ to } 35\text{ V} 26 to 35 V ), high current exceeding the transition threshold current ( I > I transition I > I_{\text{transition}} I > I transition ). Requires an argon-rich shielding gas (minimum 80 % Ar 80\%\text{ Ar} 80% Ar , balanced with CO 2 \text{CO}_2 CO 2 or O 2 \text{O}_2 O 2 ).
Physics: Electromagnetic Lorentz forces propel hundreds of tiny, sub-wire-diameter droplets axially across the arc gap per second. Creates a stable, quiet, hiss-like arc, deep "finger" root penetration, high deposition rates, and a large, fluid weld pool. Restricted to the 1G and 2F positions due to puddle fluidity.
Pulsed Spray Transfer (GMAW-P):
Operating Parameters: Advanced inverter power sources rapidly pulse current between a low background level ( I background I_{\text{background}} I background , maintaining arc stability without melting) and a high peak level ( I peak I_{\text{peak}} I peak , exceeding spray transition threshold).
Physics: Exactly one tiny molten droplet is detached per pulse. Delivers the metallurgical cleanliness, penetration, and spatter-free quality of spray transfer at an average current and heat input low enough to permit all-position welding (3G vertical and 4G overhead).
Paragraph QW-409.2: Essential Transfer Mode Rule
Code Mandate (QW-409.2): "A change from globular, spray, or pulsed spray transfer to short-circuiting transfer mode, or vice versa, is an essential variable."
Why does Section IX group globular, spray, and pulsed spray together on one side, and isolate short-circuiting on the other? Because globular, spray, and pulsed spray are all free-flight arc transfer modes with sufficient thermal energy to ensure base metal fusion. Short-circuiting is a contact transfer mode with severely reduced thermal energy and extreme cold-lap vulnerability. Shifting between free-flight and short-circuiting demands complete PQR requalification!
4. The Two Short-Circuiting Thickness Limitations: QW-403.10 and QW-404.32
Under standard ASME Section IX rules (Table QW-451.1), a procedure test coupon qualifies a maximum base metal thickness equal to twice the coupon thickness ( T max = 2 T T_{\text{max}} = 2T T max = 2 T ) and a maximum deposit of 2 t 2t 2 t . Because of the cold-lap hazard inherent in low-heat-input short-circuiting arcs, Section IX narrows both envelopes — but through two different paragraphs, each with its own subject.
The Two Statutory Mandates +----------------------------------------------------------------------------------------------------+
- | GMAW SHORT-CIRCUITING THICKNESS RULES (QW-403.10 / QW-404.32) |
- +----------------------------------------------------------------------------------------------------+
- | WHAT IS MEASURED | TRIGGER | QUALIFIED MAX | GOVERNING RULE |
- +----------------------------------------+--------------------------+---------------+-----------------+
- | Base metal thickness T of the coupon | T < 1/2 in. (13 mm) | 1.1T | QW-403.10 |
- | Base metal thickness T of the coupon | T >= 1/2 in. (13 mm) | 2T | Table QW-451.1 |
- | Deposited weld metal thickness t | t < 1/2 in. (13 mm) | 1.1t | QW-404.32 |
- | Deposited weld metal thickness t | t >= 1/2 in. (13 mm) | 2t | Table QW-451.1 |
- +----------------------------------------------------------------------------------------------------+
When a GMAW PQR is welded using short-circuiting transfer:
QW-403.10 governs the base metal. If coupon thickness T < 1 / 2 in. T < 1/2\text{ in.} T < 1/2 in. ( 13 mm 13\text{ mm} 13 mm ), the maximum base metal thickness qualified is 1.1 T 1.1T 1.1 T .
QW-404.32 governs the deposit. If the deposited weld metal thickness t < 1 / 2 in. t < 1/2\text{ in.} t < 1/2 in. ( 13 mm 13\text{ mm} 13 mm ), the maximum qualified deposit is 1.1 t 1.1t 1.1 t .
Once the relevant value reaches 1 / 2 in. 1/2\text{ in.} 1/2 in. ( 13 mm 13\text{ mm} 13 mm ) or more, the procedure has demonstrated the ability to fuse heavy sections without cold lap, and the standard 2 T 2T 2 T / 2 t 2t 2 t envelopes of Table QW-451.1 return.
- Warning
- Attribution matters on this exam. Writing "QW-404.32 limits base metal thickness to 1.1T" is the single most
- common error candidates carry into the endorsement. QW-404.32 is a QW-404 filler metal variable and therefore
governs deposited weld metal; QW-403.10 is a QW-403 base metal variable and governs base metal thickness.
Step-by-Step Mathematical Comparison
Consider two identical 0.375 in. 0.375\text{ in.} 0.375 in. ( 3 / 8 in. 3/8\text{ in.} 3/8 in. ) plate test coupons welded with ER70S-6 wire:
Coupon A (Spray Transfer): T = 0.375 in. ; Transfer Mode = Spray T = 0.375\text{ in.}; \quad \text{Transfer Mode} = \text{Spray} T = 0.375 in. ; Transfer Mode = Spray Governing Code: Table QW-451.1 applies directly: T min = 1 / 16 in. = 0.0625 in. ; T max = 2 T = 2 × 0.375 in. = 0.750 in. ( 19 mm ) T_{\text{min}} = 1/16\text{ in.} = 0.0625\text{ in.}; \quad T_{\text{max}} = 2T = 2 \times 0.375\text{ in.} = 0.750\text{ in.} (19\text{ mm}) T min = 1/16 in. = 0.0625 in. ; T max = 2 T = 2 × 0.375 in. = 0.750 in. ( 19 mm )
Coupon B (Short-Circuiting Transfer - GMAW-S): T = 0.375 in. ; Transfer Mode = Short-Circuiting T = 0.375\text{ in.}; \quad \text{Transfer Mode} = \text{Short-Circuiting} T = 0.375 in. ; Transfer Mode = Short-Circuiting Governing Code: Paragraph QW-403.10 overrides Table QW-451.1 for base metal because T = 0.375 in. < 0.500 in. T = 0.375\text{ in.} < 0.500\text{ in.} T = 0.375 in. < 0.500 in. , and paragraph QW-404.32 overrides it for the deposit because t = 0.375 in. < 0.500 in. t = 0.375\text{ in.} < 0.500\text{ in.} t = 0.375 in. < 0.500 in. T min = 1 / 16 in. = 0.0625 in. T_{\text{min}} = 1/16\text{ in.} = 0.0625\text{ in.} T min = 1/16 in. = 0.0625 in. T max = 1.1 T = 1.1 × 0.375 in. = 0.4125 in. ( 10.5 mm ) [ QW-403.10 ] T_{\text{max}} = 1.1T = 1.1 \times 0.375\text{ in.} = 0.4125\text{ in.} (10.5\text{ mm}) \quad [\text{QW-403.10}] T max = 1.1 T = 1.1 × 0.375 in. = 0.4125 in. ( 10.5 mm ) [ QW-403.10 ] t max = 1.1 t = 1.1 × 0.375 in. = 0.4125 in. ( 10.5 mm ) [ QW-404.32 ] t_{\text{max}} = 1.1t = 1.1 \times 0.375\text{ in.} = 0.4125\text{ in.} (10.5\text{ mm}) \quad [\text{QW-404.32}] t max = 1.1 t = 1.1 × 0.375 in. = 0.4125 in. ( 10.5 mm ) [ QW-404.32 ]
EXAM AUDIT ALERT: Notice that Coupon B qualifies a maximum thickness of only 0.4125 in. 0.4125\text{ in.} 0.4125 in. , compared to 0.750 in. 0.750\text{ in.} 0.750 in. for Coupon A! A production joint of 0.500 in. 0.500\text{ in.} 0.500 in. ( 1 / 2 in. 1/2\text{ in.} 1/2 in. ) wall thickness welded with GMAW-S would be illegal if supported by Coupon B, but fully legal if supported by Coupon A.
5. Filler Metal Variables: F-Numbers, A-Numbers, and Product Form (QW-404.23)
Filler metal compliance under Table QW-255 requires rigorous tracking across multiple subsections of QW-404:
F-Number (QW-404.4) and A-Number (QW-404.5)
F-Number (QW-404.4): Solid carbon steel GMAW wires (ER70S-X) and carbon steel FCAW wires (E7XT-X) are both categorized as F-No. 6 under Table QW-432. Stainless steel solid and flux-cored wires are categorized as F-No. 6 or F-No. 4X .
A-Number (QW-404.5): Dictates the chemical composition of the as-deposited weld metal. For plain carbon steels, both solid and flux-cored deposits typically qualify as A-No. 1 . A change from one A-Number to another (or to an unlisted chemistry) is an essential variable.
The Product Form Essential Variable: QW-404.23
One of the most frequent traps in code compliance audits is the assumption that because ER70S-6 solid wire and E71T-1M flux-cored wire are both F-No. 6, A-No. 1 electrodes, a fabricator can freely substitute them on a WPS without requalification. This is completely false!
Paragraph QW-404.23 states:
"A change from one of the following filler metal product forms to another: (a) bare (solid) or metal cored to flux cored, or vice versa; (b) flux cored to bare (solid) or metal cored; or (c) powder to solid or cored wire is an essential variable." +----------------------------------------------------------------------------------------------------+
- | PRODUCT FORM PERMUTATIONS (QW-404.23) |
- +----------------------------------------------------------------------------------------------------+
- | ORIGINAL PQR CONSUMABLE | PROPOSED WPS CONSUMABLE | CODE STATUS |
- +-----------------------------------+-----------------------------------+----------------------------+
- | GMAW Solid Wire (ER70S-6) | MCAW Metal-Cored (E70C-6M) | Permitted without new PQR* |
- | GMAW Solid Wire (ER70S-6) | FCAW Flux-Cored (E71T-1M) | REQUALIFICATION REQUIRED |
- | FCAW Flux-Cored (E71T-1M) | GMAW Solid Wire (ER70S-6) | REQUALIFICATION REQUIRED |
- | FCAW-G Dual Shield (E71T-1M) | FCAW-S Self-Shielded (E71T-8) | REQUALIFICATION REQUIRED** |
- +----------------------------------------------------------------------------------------------------+
*Note: Bare solid and metal-cored wires belong to the same product form grouping under QW-404.23(a).
**Note: Eliminating shielding gas is also an essential variable under QW-408.1.
Metallurgical Differences Driving QW-404.23
Why does the code enforce this barrier? Solid wire deposits 100% metallic alloy with minimal deoxidation slag. Flux-cored wire introduces extensive slag-metal reactions, complex deoxidizers (aluminum, magnesium, titanium), and potential inclusions that affect mechanical properties, grain morphology, and hydrogen cracking susceptibility.
6. Shielding Gas Variables: Composition Shifts & Purging (QW-408)
Table QW-255 establishes tight boundaries on the gaseous environment shielding the arc:
Addition or Deletion of Gas (QW-408.1)
Adding shielding gas to a self-shielded process, or deleting shielding gas from a gas-shielded process, is an essential variable .
The 5% Composition Shift Rule (QW-408.2)
Under paragraph QW-408.2 , an essential variable is triggered by:
A change from a single shielding gas to any other single shielding gas (e.g., 100 % CO 2 100\%\text{ CO}_2 100% CO 2 to 100 % Ar 100\%\text{ Ar} 100% Ar ).
A change from a single shielding gas to a mixture of gases, or vice versa (e.g., 100 % CO 2 100\%\text{ CO}_2 100% CO 2 to 75 % Ar / 25 % CO 2 75\%\text{ Ar} / 25\%\text{ CO}_2 75% Ar /25% CO 2 ).
A change in the specified nominal percentage composition of a shielding gas mixture of greater than 5 % 5\% 5% . +----------------------------------------------------------------------------------------------------+
- | THE 5% SHIELDING GAS SHIFT THRESHOLD |
- +----------------------------------------------------------------------------------------------------+
- | QUALIFIED PQR GAS BLEND | PROPOSED PRODUCTION GAS BLEND | EVALUATION & STATUS |
- +--------------------------------+----------------------------------+--------------------------------+
- | 75% Ar / 25% CO2 | 80% Ar / 20% CO2 | Ar +5%, CO2 -5% -> BORDERLINE |
- | 75% Ar / 25% CO2 | 85% Ar / 15% CO2 | Ar +10%, CO2 -10% -> REQUALIFY |
- | 98% Ar / 2% O2 | 95% Ar / 5% O2 | O2 shift +3% <= 5% -> WPS REV |
- | 90% He / 7.5% Ar / 2.5% CO2 | 80% He / 15% Ar / 5% CO2 | He -10% (> 5%) -> REQUALIFY |
- +----------------------------------------------------------------------------------------------------+
- Backing Gas and Purging Rules (QW-408.5 & QW-408.8)
For complete penetration groove welds in piping and pressure vessels:
QW-408.5: The addition or deletion of backing gas is an essential variable .
QW-408.8: The deletion of backing gas, or a decrease in backing gas flow rate, is an essential variable .
- 7. Electrical Characteristics: Polarity and Heat Input (QW-409)
- Polarity and Current Type (QW-409.4)
A change from AC to DC, or a change in polarity from DCEP (Electrode Positive) to DCEN (Electrode Negative) , is an essential variable .
Solid wire GMAW and gas-shielded FCAW-G almost exclusively utilize DCEP , which concentrates electron bombardment on the cathode (the base metal workpiece), producing cleaning action, stable arc physics, and deep penetration.
Many self-shielded FCAW-S wires (such as AWS E71T-8 and E71T-11) require DCEN . In DCEN, electron bombardment concentrates heat at the wire tip, dramatically increasing burn-off rate while minimizing heat input into thin sheet metal. Operating an FCAW-S wire on DCEP causes severe arc instability, porosity, and embrittlement.
Heat Input (QW-409.1)
An increase in heat input or weld metal volume per unit length is a supplementary essential variable , triggered whenever construction codes (ASME Section VIII, B31.3 low-temperature) mandate notch-toughness testing.