Study guide

8.2 Submerged Arc Welding (SAW) Procedure Variables and Flux-Wire Combinations

AWS ASME BPVC Section IX + B31.1/B31.3 Endorsement CWI/SCWI

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: Exam Structure, Logistics & Code Navigation Strategy

1.1 Credential Overview, Prometric Delivery & July 2025 Hard-Copy Rule 1.2 The Three-Code Triad: Section IX, B31.1, and B31.3 Roles & Interrelationships 1.3 Rapid Code-Book Navigation: Tabbing, Cross-Referencing & Time Management

2 Chapter 2: Section IX Article I — General Welding Requirements

2.1 Scope, Responsibilities & Section IX Architecture 2.2 Mechanical Test Types, Specimen Dimensions & Acceptance Criteria 2.3 Notch-Toughness Tests, Fillet-Weld Tests & Special Examinations

3 Chapter 3: Section IX Article II — Procedure Qualification Fundamentals

3.1 PQR vs. WPS Workflow, Purpose & Content Requirements 3.2 Coupling and Supporting Multiple WPSs and PQRs 3.3 Test Coupons, Preparation & Required Test Specimen Allocations

4 Chapter 4: Section IX Procedure Qualification Limits & Thickness Rules

4.1 Base Metal & Deposited Weld Metal Thickness Limits 4.2 Impact Testing Requirements & Toughness Thickness Qualification Ranges 4.3 Fillet Weld Procedure Qualification Rules & Special Applications

5 Chapter 5: Section IX Article III — Welder Performance Qualification Fundamentals

5.1 Welder & Welding Operator Qualification Intent, Responsibilities & Identification 5.2 Qualification Testing Methods: Mechanical Bend Tests vs. Volumetric NDE 5.3 Welder Qualification Continuity, Expiration, and Requalification

6 Chapter 6: Section IX Welder Performance Limits, Positions & Diameters

6.1 Test Positions, Groove Weld Orientations & Production Position Limits 6.2 Welder Thickness Limits and Pipe Diameter Qualification Ranges 6.3 Welder Essential Variables: F-Numbers, Backing, and Process Transfers

7 Chapter 7: Section IX Article IV — Welding Variables by Process (Part 1: SMAW & GTAW)

7.1 Understanding Essential, Supplementary Essential & Nonessential Variables 7.2 Shielded Metal Arc Welding (SMAW) Procedure Variables 7.3 Gas Tungsten Arc Welding (GTAW) Procedure Variables

8 Chapter 8: Section IX Article IV — Welding Variables by Process (Part 2: GMAW/FCAW & SAW)

8.1 GMAW & FCAW Procedure Variables and Short-Circuiting Transfer Rules 8.2 Submerged Arc Welding (SAW) Procedure Variables and Flux-Wire Combinations 8.3 Special Variables: Heat Input, Electrical Characteristics & Shielding Gases

9 Chapter 9: Section IX Material Classifications, Numbers & Standard Documentation

9.1 Base Metal P-Numbers, Group Numbers, and S-Numbers 9.2 Filler Metal F-Numbers and As-Deposited Chemistry A-Numbers 9.3 ASME Standard Documentation: Auditing WPS, PQR, and WPQ Forms

10 Chapter 10: ASME B31.1 Power Piping — Scope, Materials, Design & Welding Fabrication

10.1 B31.1 Scope, Jurisdiction, Boiler External Piping vs. Non-Boiler External Piping 10.2 B31.1 Welding Requirements, Joint Alignment, Backing Rings & Tack Welds 10.3 B31.1 Welder & Procedure Qualification Interfacing with Section IX 10.4 B31.1 Materials, Design Conditions & Pressure Design of Components

11 Chapter 11: ASME B31.1 Power Piping — Heat Treatment, Examination, Testing & Fabrication Records

11.1 B31.1 Preheat Rules & Mandatory Temperatures 11.2 B31.1 Postweld Heat Treatment (PWHT) Rules, Temperatures & Holding Times 11.3 B31.1 Mandatory NDE Examination, Acceptance Standards & Pressure Leak Tests 11.4 B31.1 Bending, Forming, Assembly & Code Records

12 Chapter 12: ASME B31.3 Process Piping — Scope, Fluid Services, Materials, Design & Welding

12.1 B31.3 Scope, Fluid Service Classifications & Owner Responsibilities 12.2 B31.3 Welding, Joint Preparation, Backing Rings & Fabrication Details 12.3 B31.3 Procedure & Performance Qualification Rules and Section IX Exceptions 12.4 B31.3 Materials, Design Conditions & Pressure Design of Components

13 Chapter 13: ASME B31.3 Process Piping — Heat Treatment, Examination, Testing, Fabrication & Records

13.1 B31.3 Preheat and Postweld Heat Treatment Rules & Tables 13.2 B31.3 Inspection vs. Examination Responsibilities & Examination Extents 13.3 B31.3 Acceptance Criteria for Weld Imperfections 13.4 B31.3 Pressure Leak Testing: Hydrostatic, Pneumatic & Sensitive Leak Tests 13.5 B31.3 Bending, Forming, Assembly & Records

8.2 Submerged Arc Welding (SAW) Procedure Variables and Flux-Wire Combinations

Key Takeaways Explain This Topic AI

Under Table QW-258 and paragraph QW-404.9, a change in the flux trade name or the AWS classification of the flux-wire combination is an essential variable requiring procedure requalification.

Under paragraph QW-404.36, the addition or deletion of crushed slag (reground slag), or any change in the ratio of virgin flux to reground slag, is an essential variable.

A change from a single electrode to multiple electrodes (such as tandem or twin wire systems), or vice versa, is an essential variable per QW-410.9.

Under paragraph QW-404.24, the addition or deletion of supplemental filler metal (cold wire feed, cut wire, or iron powder) is an essential variable.

Active fluxes contribute manganese and silicon to the weld deposit, which can cause brittle alloy buildup in multi-pass welds; a change from neutral to active flux is an essential variable under QW-404.34.

Last updated: September 2026

8.2 Submerged Arc Welding (SAW) Procedure Variables and Flux-Wire Combinations

Core Principle: Submerged Arc Welding (SAW) is an automated, high-deposition process where an electric arc burns invisibly beneath a thick, protective blanket of granular, fusible flux. Unlike gas-shielded or manual processes where wire and shielding are evaluated independently, ASME Section IX Table QW-258 treats the SAW flux and consumable electrode as an indivisible chemical and metallurgical couple. Changes to flux classification (QW-404.9), slag recycling practices (QW-404.36), multi-electrode configurations (QW-410.9), or supplemental cold wire additions (QW-404.24) represent essential variables that alter weld pool chemistry and demand full procedure requalification.

1. Table QW-258 Architecture and SAW Operational Physics

Submerged Arc Welding operates at extremely high electrical currents ( 300 to 1500 + A 300\text{ to } 1500+\text{ A} 300 to 1500 + A ), delivering deposition rates of 10 to 60 + lb/hr 10\text{ to } 60+\text{ lb/hr} 10 to 60 + lb/hr with thermal efficiencies exceeding 85 % to 90 % 85\%\text{ to } 90\% 85% to 90% . The molten flux blanket performs three indispensable roles:

Atmospheric Shielding: Melts into a conductive liquid slag barrier that completely excludes oxygen, nitrogen, and ambient humidity from the superheated molten pool.

Electrochemical Refining & Deoxidation: Reacts with dissolved oxides in the puddle, scavenging impurities into the floating slag via manganese ( M n Mn M n ), silicon ( S i Si S i ), and calcium fluoride ( C a F 2 CaF_2 C a F 2 ​ ) additions.

Thermal Insulation & Bead Shaping: Retards the cooling rate of the weld pool, promoting smooth bead transitions and facilitating the escape of entrapped gases. +----------------------------------------------------------------------------------------------------+

  • | SUBMERGED ARC WELDING (SAW) SCHEMATIC |
  • +----------------------------------------------------------------------------------------------------+
  • | [Consumable Bare Wire Electrode (Continuous Spool)] |
  • | | |
  • | v (Motorized Wire Feed Rolls) |
  • | [Contact Tip / Jaw] |
  • | | |
  • | [Granular Flux Blanket] v (Arc Current 300 - 1500 A) |
  • | ~~~~~~~~~~~~~~~~~~~~~~~~(Submerged Arc)~~~~~~~~~~~~~~~~~~~~~~~~ |
  • | [Solidified Slag] -> (====== Molten Slag ======) |
  • | [Weld Metal Bead] -> (=== Molten Weld Pool ===) |
  • | =====================[Base Metal Workpiece]===================== |
  • +----------------------------------------------------------------------------------------------------+
  • 2. Table QW-258 Variable Classification Matrix

Inspectors and engineers preparing for the CWI endorsement exam must know every variable in Table QW-258 and its exact classification:

  • Variable Category Paragraph Variable Description Variable Status
  • Joints (QW-402) QW-402.1 Deletion of backing Nonessential
  • QW-402.4 Change in groove cross-section / bevel angle Nonessential
  • QW-402.10 Change in root spacing Nonessential
  • QW-402.11 Addition or deletion of retainers Nonessential
  • Base Metals (QW-403) QW-403.5 Change in base metal Group Number (toughness) Supplementary Essential
  • QW-403.6 Minimum base metal thickness T T T qualified (toughness) Supplementary Essential
  • QW-403.8 Change in base metal thickness T T T qualified per QW-451 Essential

QW-403.9 Single-pass weld deposit t > 1 / 2 in. t > 1/2\text{ in.} t > 1/2 in. ( 13 mm 13\text{ mm} 13 mm ) Essential

  • Filler Metals (QW-404) QW-404.4 Change in F-Number Essential
  • QW-404.5 Change in A-Number Essential
  • QW-404.9 Change in flux-wire classification or flux trade name Essential
  • QW-404.10 Change in manufacturer / trade name of alloy flux Essential
  • QW-404.24 Addition or deletion of supplemental filler metal Essential
  • QW-404.30 Change in deposited thickness t t t per QW-451 Essential
  • QW-404.34 Change in flux type (neutral to active, or vice versa) Essential
  • QW-404.35 Change in flux trade name (for unclassified combinations) Essential
  • QW-404.36 Addition, deletion, or ratio change of crushed slag Essential
  • Positions (QW-405) QW-405.1 Addition of positions (SAW restricted to 1G/1F/2F) Nonessential

Preheat (QW-406) QW-406.1 Decrease of > 100 ∘ F > 100^\circ\text{F} > 10 0 ∘ F ( 55 ∘ C 55^\circ\text{C} 5 5 ∘ C ) in preheat Essential

QW-406.3 Increase of > 100 ∘ F > 100^\circ\text{F} > 10 0 ∘ F ( 55 ∘ C 55^\circ\text{C} 5 5 ∘ C ) in interpass temp Supplementary Essential

  • PWHT (QW-407) QW-407.1 Change in PWHT condition Essential
  • QW-407.2 Change in PWHT time and temperature cycle Supplementary Essential

Electrical (QW-409) QW-409.1 Increase in heat input or volume of deposit per unit length Supplementary Essential

  • QW-409.4 Change in current type (AC/DC) or polarity (DCEP/DCEN) Essential
  • QW-409.8 Change in amperage, voltage, or travel speed range Nonessential
  • Technique (QW-410) QW-410.1 Change from string to weave bead Nonessential
  • QW-410.5 Method of initial and interpass cleaning Nonessential
  • QW-410.6 Method of back gouging Nonessential
  • QW-410.7 Change from single to multiple electrodes (or vice versa) Essential
  • QW-410.8 Change from single to multi-pass per side Supplementary Essential
  • QW-410.9 Change in electrode spacing or alignment in multi-wire Essential
  • QW-410.10 Change from single to multi-pass per side (toughness) Supplementary Essential
  • QW-410.15 Change in flux brand or commercial designation Essential
  • 3. The Flux-Wire Combination: Inseparable Metallurgical Coupling (QW-404.9)

In SMAW or GTAW, an electrode specification (e.g., SFA-5.1 E7018 or SFA-5.18 ER70S-6) defines mechanical properties independently of any external flux brand. In SAW, an electrode wire alone has no certified tensile, yield, or impact properties!

AWS SFA-5.17 / SFA-5.23 Classification System

Mechanical integrity is certified exclusively for the flux-wire combination as a unified system under AWS A5.17 (carbon steel) or AWS A5.23 (low-alloy steel): F 7 A 2 − E M 12 K \mathbf{F7A2-EM12K} F7A2 − EM12K

F: Submerged Arc Welding Flux

7: Minimum tensile strength in increments of 10 ksi 10\text{ ksi} 10 ksi ( 70 to 95 ksi 70\text{ to } 95\text{ ksi} 70 to 95 ksi , or 480 to 650 MPa 480\text{ to } 650\text{ MPa} 480 to 650 MPa )

A: As-welded condition (P indicates Postweld Heat Treated condition)

2: Minimum Charpy V-notch impact toughness of 20 ft-lbf 20\text{ ft-lbf} 20 ft-lbf at − 20 ∘ F -20^\circ\text{F} − 2 0 ∘ F ( − 29 ∘ C -29^\circ\text{C} − 2 9 ∘ C )

  • E: Electrode (wire)
  • M: Medium manganese content ( 0.80 % to 1.25 % Mn 0.80\%\text{ to } 1.25\%\text{ Mn} 0.80% to 1.25% Mn )
  • 12: Nominal carbon content in hundredths of a percent ( 0.12 % C 0.12\%\text{ C} 0.12% C )
  • K: Produced from killed (fully deoxidized) steel
  • The QW-404.9 Essential Variable Rule

Under paragraph QW-404.9 , an essential variable is triggered by:

A change in the indicator for flux-wire classification (e.g., from F7A2-EM12K to F7A4-EM12K, or from F7A2-EM12K to F7P2-EM12K).

A change in the wire manufacturer or trade name when using unclassified or proprietary fluxes.

A change in flux manufacturer trade name, even when the AWS classification designation remains identical!

CRITICAL CODE DISTINCTION: Unlike bare wire in GMAW or GTAW (where an ER70S-6 wire from Manufacturer A can be substituted with ER70S-6 from Manufacturer B under the same WPS), you cannot swap flux brands in SAW without qualifying a new PQR! A Lincoln 761 flux combined with Lincoln L-61 wire cannot be replaced by an ESAB OK 10.71 flux and OK 12.22 wire without a new procedure qualification test coupon, even if both combinations are certified as F7A2-EM12K.

Neutral vs. Active Fluxes (QW-404.34)

Neutral Fluxes: Formulated with a balanced chemical basicity index ( B I ≈ 1.2 to 2.5 BI \approx 1.2\text{ to } 2.5 B I ≈ 1.2 to 2.5 ). They do not significantly alter the manganese or silicon content of the weld deposit, regardless of changes in arc voltage or pass count. Essential for heavy-section, multi-pass groove welds where deposit chemistry must remain constant from root to cap.

Active Fluxes: Contain intentional additions of manganese and silicon deoxidizers. They resist porosity when welding over mill scale, light rust, and oil on single-pass or two-pass fillet/groove applications. However, in multi-pass welds, each subsequent pass introduces cumulative manganese and silicon buildup. This causes uncontrolled hardening ( > 300 HB > 300\text{ HB} > 300 HB ), severe embrittlement, and centerline cracking.

Code Rule (QW-404.34): A change from a neutral flux to an active flux, or vice versa, is an essential variable .

4. Crushed Slag and Recycled Flux Rules: Paragraph QW-404.36

In high-volume SAW operations (pipe mills, structural beam fabrication, shipyards), vast quantities of glassy, solidified slag are ejected as the weld bead cools. Historically, fabricators attempted to crush, regrind, and blend this waste slag back into virgin flux hoppers to cut consumable costs.

Metallurgical Degradation from Crushed Slag

When granular virgin flux is melted in the arc, vital thermodynamic reactions occur:

Deoxidizing elements (Mn, Si, Ti, Al) react with oxygen in the molten puddle and are consumed, forming stable oxides ( M n O MnO M n O , S i O 2 SiO_2 S i O 2 ​ ) that partition into the slag.

Volatile fluoride compounds ( C a F 2 CaF_2 C a F 2 ​ ) vaporize, altering arc stability and slag detachment characteristics.

Tramp impurities from the plate surface (sulfur, phosphorus, mill scale, moisture) are absorbed into the slag structure.

When this exhausted slag is pulverized and reused, the resulting flux mixture is depleted of active deoxidizers and enriched in oxides and contaminants . Re-welding with crushed slag yields coarse columnar microstructures, catastrophic loss of low-temperature Charpy V-notch toughness, and elevated porosity.

The QW-404.36 Statutory Mandate +----------------------------------------------------------------------------------------------------+

  • | PARAGRAPH QW-404.36 REGROUND SLAG RESTRICTION |
  • +----------------------------------------------------------------------------------------------------+
  • | FABRICATION ACTION | ASME SECTION IX CODE STATUS |
  • +--------------------------------------------------------+-------------------------------------------+
  • | Addition of crushed / reground slag | ESSENTIAL VARIABLE (Requalification Req.) |
  • | Deletion of crushed / reground slag | ESSENTIAL VARIABLE (Requalification Req.) |
  • | Change in ratio of virgin flux to crushed slag | ESSENTIAL VARIABLE (Requalification Req.) |
  • +--------------------------------------------------------+-------------------------------------------+

Exam Trap: An exam question might ask: "A manufacturer adds 20% reground crushed slag to virgin SAW flux. Is this acceptable?" The answer: It is an essential variable under QW-404.36. The manufacturer must weld a PQR coupon using that exact 20% blend, pass all tension and bend tests, and document the specific crushed slag ratio on the PQR and WPS. Crushed slag cannot be introduced into an existing virgin-flux WPS without requalification!

5. Multi-Wire vs Single-Wire Arc Systems (QW-410.7 & QW-410.9)

To achieve massive deposition rates ( 40 to 80 + lb/hr 40\text{ to } 80+\text{ lb/hr} 40 to 80 + lb/hr ) in spiral pipe mills and heavy pressure vessel girth seams, SAW systems frequently employ multiple wire electrodes operating in a single molten puddle or in closely spaced tandem puddles.

Arc Configurations

Single-Wire SAW: One continuous electrode feeding into the arc zone ( 300 to 800 A 300\text{ to } 800\text{ A} 300 to 800 A ).

Twin-Wire SAW (Parallel Arc): Two wires fed simultaneously through a single contact tip powered by a single power source. Delivers higher deposition at lower current density.

Tandem-Arc SAW (Multi-Power): Two or more independent wire feeds, each energized by its own dedicated power supply and contact tip:

Lead Arc: Typically powered by DCEP to ensure deep penetration at the root of the joint.

Trail Arc(s): Powered by AC (Alternating Current) . Utilizing AC on the trailing wire eliminates magnetic arc blow between adjacent arcs while filling the groove and flattening the bead profile. +----------------------------------------------------------------------------------------------------+

  • | TANDEM-ARC SAW CONFIGURATION (QW-410.9) |
  • +----------------------------------------------------------------------------------------------------+
  • | [Lead Electrode: DCEP] [Trail Electrode: AC] |
  • | (Deep Penetration) (Bead Shaping & Fill) |
  • | | | |
  • | v v |
  • | (Lead Arc Zone) <-- Spacing (S) --> (Trail Arc Zone) |
  • | ~~~~~~~~~~~~~~~~~~~~~~~~(Shared Flux Blanket)~~~~~~~~~~~~~~~~~~~~~~~~ |
  • | =====================[Heavy Plate Workpiece]========================= |
  • +----------------------------------------------------------------------------------------------------+
  • The QW-410.7 and QW-410.9 Rules

QW-410.7: A change from a single electrode to multiple electrodes, or vice versa, is an essential variable .

QW-410.9: In multiple-electrode systems, a change in electrode spacing, alignment angle, or electrical configuration (e.g., switching the trail arc from AC to DC) is an essential variable .

6. Supplemental Filler Metal Additions: Paragraph QW-404.24

In ultra-high productivity SAW applications, fabricators introduce supplemental cold metal into the arc cavity without passing current through it:

Cold Wire Addition: An auxiliary solid wire fed into the molten puddle, melted solely by excess thermal energy from the primary arc.

Iron Powder / Cut Wire Addition: Granular metallic iron or chopped alloy wire metered into the groove bevel ahead of the flux blanket.

Metallurgical Impact

Supplemental filler metal acts as an internal heatsink, absorbing arc superheat to melt. This drastically increases deposition rate ( + 30 % to + 100 % +30\%\text{ to }+100\% + 30% to + 100% ), decreases base metal dilution, narrows the coarse-grained HAZ, and speeds up weld puddle solidification.

The QW-404.24 Rule

Under paragraph QW-404.24 , the addition or deletion of supplemental filler metal is an essential variable . A PQR qualified with cold wire feed cannot support a WPS welded without cold wire, and vice versa.

7. Heavy-Deposition SAW and Table QW-451.1 Note (1)

Because SAW deposits heavy beads, candidates must cross-reference Table QW-451.1 Note (1) rules:

If a test coupon deposits weld metal t ≥ 3 / 4 in. t \ge 3/4\text{ in.} t ≥ 3/4 in. ( 19 mm 19\text{ mm} 19 mm ) using three or more layers , the maximum qualified weld metal thickness is 8.0 in. 8.0\text{ in.} 8.0 in. ( 200 mm 200\text{ mm} 200 mm ) .

If high-amperage SAW deposits t = 0.75 in. t = 0.75\text{ in.} t = 0.75 in. in only one or two massive passes , Note (1) does not apply! The maximum qualified weld metal thickness is restricted to standard 2 t = 1.50 in. 2t = 1.50\text{ in.} 2 t = 1.50 in.

Single-Pass Grain Coarsening Hazard (QW-403.9 & QW-410.8)

When SAW deposits passes thicker than 1 / 2 in. 1/2\text{ in.} 1/2 in. ( 13 mm 13\text{ mm} 13 mm ) per QW-403.9, or when single-pass welding is converted to multi-pass welding per QW-410.8, severe grain-size variations occur. In single-pass SAW, the entire weld nugget remains in the un-tempered as-cast dendritic condition, severely degrading impact toughness.

Loading diagram... Figure 8.2: Submerged Arc Welding (Table QW-258) Essential Variables