Study guide
4.3 WPS Essential Variables, Base Metal Ranges & Qualified Positions (Table 6.6)
AWS D1.1 Structural Steel Endorsement Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Exam Structure, Code Scope & General Requirements
1.1 AWS D1.1 Endorsement Exam Format & Open-Book Navigation 1.2 Clause 1 Scope, Responsibilities & Structural Classifications 1.3 Normative References, Terminology & Base Metal Scope
2 Chapter 2: Design of Welded Connections (Clause 4)
2.1 Groove and Fillet Weld Design & Effective Throat Calculations 2.2 Statically Loaded Connection Details, Geometry Limits & Transitions 2.3 Cyclically Loaded Structures, Stress Categories & Fatigue Life Design
3 Chapter 3: Prequalification of Welding Procedure Specifications (Clause 5)
3.1 Prequalified Processes, Base Metal Groups & Matching Filler Metals 3.2 Prequalified Joint Geometries, CJP/PJP Details & Backing 3.3 Prequalified Minimum Fillet Sizes & Preheat/Interpass Temperatures
4 Chapter 4: Welding Procedure Specification (WPS) Qualification (Clause 6, Part B)
4.1 WPS Qualification Requirements, PQR Coupon Testing & Mechanical Evaluation 4.2 PQR Mechanical Test Types: Tension, Guided Bend & Macroetch 4.3 WPS Essential Variables, Base Metal Ranges & Qualified Positions (Table 6.6)
5 Chapter 5: Welder, Welding Operator & Tack Welder Performance Qualification (Clause 6, Part C)
5.1 Welder Qualification Test Plates, Positions & Pipe Assemblies 5.2 Performance Test Evaluation (Visual, Guided Bend, Macroetch) & Retest Rules 5.3 Performance Essential Variables, Qualification Limits (Table 6.12) & Continuity
6 Chapter 6: Fabrication & Workmanship (Clause 7)
6.1 Base Metal Preparation, Thermal Cutting Tolerances & Fit-Up 6.2 Welding Consumable Storage, Low-Hydrogen Exposure Limits & Baking 6.3 Distortion Control, Arc Strikes, Tack Welds & Weld Repair Rules
7 Chapter 7: Visual Inspection & Acceptance Criteria (Clause 8, Parts A-C)
7.1 Inspector Responsibilities, Qualifications (CWI/SCWI) & Inspection Sequence 7.2 Table 8.1 Visual Inspection Criteria: Static vs. Cyclic Non-Tubular Connections 7.3 Weld Profiles, Undercut Tolerances, Porosity Limits & Crack Rejection
8 Chapter 8: Nondestructive Testing (NDT) Procedures & Acceptance (Clause 8, Part D)
8.1 Radiographic Testing (RT) Requirements, IQI Placement & Acceptance 8.2 Ultrasonic Testing (UT) Procedures, Calibration & Tables 8.2 / 8.3 8.3 Magnetic Particle (MT), Liquid Penetrant (PT) & Inspection Records
9 Chapter 9: Stud Welding & Tubular Structures (Clauses 9 & 10)
9.1 Clause 9 Stud Welding: Pre-Production Testing, Bend Tests & Flash Acceptance 9.2 Clause 10 Tubular Connections: T-, Y-, K-Joints, Geometry & Effective Throat 9.3 Clause 10 Tubular Qualification & Inspection: 6GR Restriction Testing & Acceptance
10 Chapter 10: Strengthening/Repair of Existing Structures & Welding Symbols (Clause 11 & AWS A2.4)
10.1 Clause 11 Evaluation, Base Metal Identification & Welding Under Load 10.2 Clause 11 Repair Workmanship, Heat Input Control & Member Restoration 10.3 AWS A2.4 Welding Symbols: Notation, Sizing, Pitch & Field Flags
4.3 WPS Essential Variables, Base Metal Ranges & Qualified Positions (Table 6.6)
Key Takeaways Explain This Topic AI
A WPS Essential Variable is any parameter change beyond codified limits that alters the mechanical properties of the weldment and legally mandates PQR requalification.
A PQR coupon welded on plate with thickness T >= 1 in. (25 mm) qualifies the WPS for all production thicknesses from 1/8 in. (3 mm) to Unlimited.
Heat input increases greater than 10% require WPS requalification whenever welding quenched and tempered steels (Group IV) or when CVN impact toughness is specified.
Qualifying a CJP groove weld in the 1G (flat) position qualifies only the flat position, whereas qualifying in 1G, 2G, 3G, and 4G positions (or 6G pipe) qualifies the WPS for all positions.
A change in vertical welding progression between vertical-up and vertical-down is a non-negotiable essential variable requiring complete procedure requalification.
Last updated: August 2026
WPS Essential Variables Framework (Table 6.6)
An Essential Variable is a welding parameter, material property, or joint characteristic which, if modified beyond the specific tolerances established in AWS D1.1 Table 6.6 , could adversely affect the mechanical properties, soundness, or metallographic structure of the welded joint. Any change exceeding an essential variable tolerance immediately invalidates the WPS and mandates requalification through a new PQR . +-----------------------------------------------------------------------------------------+
- | WPS ESSENTIAL VARIABLE REQUALIFICATION TRIGGERS |
- +-----------------------------------------------------------------------------------------+
- | |
- | +------------------------+ +------------------------+ +---------------------------+ |
- | | PROCESS & METALS | | ELECTRICAL & HEAT | | POSITION & GEOMETRY | |
- | +------------------------+ +------------------------+ +---------------------------+ |
- | | * Change in process | | * Heat input > +10% | | * Change in position | |
- | | * Change in Base Group | | (for Q&T or CVN) | | * Progression: Up vs Down | |
- | | * Change in F-Number | | * Current: > +/- 10-15%| | * Omission of backing | |
- | | * Change in Gas Ratio | | * Voltage: > +/- 7-10% | | * Change in Groove Type | |
- | | (> 5% Ar/CO2 shift) | | * Travel Speed: > 15% | | * Root opening decrease | |
- | +------------------------+ +------------------------+ +---------------------------+ |
- | |
- +-----------------------------------------------------------------------------------------+
- Master Summary of Table 6.6 Essential Variable Changes
- Variable Category Essential Variable Change Requiring WPS Requalification Applicable Processes
- Welding Process Any change from one welding process to another, or combination of processes. All Processes
Base Metal 1. Change from one Base Metal Group (Table 5.6) to another.; 2. Welding an unlisted steel not qualified on the PQR.; 3. Change in base metal thickness (T) outside Table 6.2 limits. All Processes
Filler Metal 1. Increase in filler metal strength classification (e.g., E7018 to E8018).; 2. Change in AWS electrode classification F-number or A-number.; 3. Change in electrode nominal diameter by more than permitted. SMAW, GMAW, FCAW, SAW
Shielding Gas 1. Change in nominal shielding gas composition (> 5% variation in major component).; 2. Decrease in gas flow rate > 25% or increase > 50%.; 3. Change from single gas to mixture or vice versa. GMAW, FCAW-G, GTAW
Electrical Variables 1. Change in current type (AC vs. DC) or polarity (DCEP vs. DCEN).; 2. Amperage change outside ±10% to ±15%.; 3. Voltage change outside ±7% to ±10%.; 4. Travel speed change outside ±15%. All Processes
Position & Progression 1. Addition of welding positions not qualified by Table 6.1.; 2. Change in vertical progression from vertical-up to vertical-down or vice versa. All Processes
- Electrical Variables & Heat Input Control (Clause 6.8, Table 6.6 & Table 6.8)
- Heat Input Calculation Formula
Heat input represents the quantity of electrical energy delivered to the weldment per unit length of weld seam. It directly controls cooling rates, microstructural phase transformations, HAZ grain size, and mechanical toughness. H = (60 × E × I) / (1000 × S)
Where:
- H = Heat input in kilojoules per inch (kJ/in.) [or kJ/mm if divided by S in mm/min]
- E = Arc voltage (Volts)
- I = Welding current (Amperes)
- S = Travel speed of the arc (inches per minute [ipm] or mm/min)
- 60 = Conversion constant (seconds per minute)
- 1000 = Conversion constant (Joules to kiloJoules)
- The > 10% Heat Input Rule for Toughness & Q&T Steels
AWS D1.1 Table 6.8 (supplementary essential variables for CVN applications) makes an increase of greater than 10% in heat input over the value recorded on the PQR an essential variable requiring procedure requalification , and Clause 7.7 separately caps heat input on quenched and tempered steels. This applies whenever:
The procedure is applied to Group IV quenched and tempered steels (e.g., ASTM A514, A517, ASTM A709 Grades 100/100W).
Charpy V-Notch (CVN) impact toughness is specified in contract documents for any base metal. +-----------------------------------------------------------------------------------------+
- | WORKED HEAT INPUT EVALUATION EXAMPLE |
- +-----------------------------------------------------------------------------------------+
- | |
- | PQR Recorded Parameters (ASTM A514 Plate): |
- | * Current (I) = 220 A |
- | * Voltage (E) = 26 V |
- | * Travel Speed (S) = 12.0 ipm |
- | * PQR Heat Input: H_pqr = (60 * 26 * 220) / (1000 * 12.0) = 28.60 kJ/in. |
- | * Maximum Allowable Heat Input (+10% Limit): 28.60 * 1.10 = 31.46 kJ/in. |
- | |
- | PROPOSED PRODUCTION WPS SETTINGS: |
- | * Proposed Current = 250 A, Voltage = 28 V, Travel Speed = 11.0 ipm |
- | * Calculated WPS Heat Input: H_wps = (60 * 28 * 250) / (1000 * 11.0) = 38.18 kJ/in. |
- | * Evaluation: 38.18 kJ/in. > 31.46 kJ/in. (+33.5% increase) |
- | * RESULT: REJECTED. Mandates complete procedure requalification via a new PQR. |
- | |
- +-----------------------------------------------------------------------------------------+
- Position Qualification Rules & Qualified Thickness Ranges (Tables 6.1 & 6.2)
- Position Qualification Matrix for Plate Groove Welds
In WPS qualification, testing in a specific position qualifies the procedure for specific production welding positions according to Table 6.1: +-----------------------------------------------------------------------------------------+
- | WPS POSITION QUALIFICATION RULES (TABLE 6.1) |
- +-----------------------------------------------------------------------------------------+
- | |
- | PQR TEST POSITION QUALIFIED PRODUCTION POSITIONS |
- | ============================================================================= |
- | 1G (Flat Position) ---> Flat (1G) Groove & Flat (1F) Fillet only |
- | 2G (Horizontal Position) ---> Flat (1G) & Horizontal (2G) Groove; 1F & 2F Fillet|
- | 3G (Vertical Position) ---> Flat (1G) & Vertical (3G) Groove; 1F, 2F, 3F Fillet|
- | 4G (Overhead Position) ---> Flat (1G) & Overhead (4G) Groove; 1F, 2F, 4F Fillet|
- | |
- | ALL-POSITION QUALIFICATION: |
- | * Requires testing coupons in 1G, 2G, 3G, and 4G positions (or 2G + 3G + 4G), OR |
- | * Qualifying on a 6G pipe test assembly per Table 10.8. |
- | |
- +-----------------------------------------------------------------------------------------+
- Qualified Thickness Ranges for CJP Plate Coupons (Table 6.2)
AWS D1.1 Table 6.2 establishes the qualified base metal thickness range (T) based on the nominal thickness of the PQR test plate:
- PQR Test Plate Thickness (T) Minimum Qualified Thickness Maximum Qualified Thickness
- 1/8 in. ≤ T < 3/8 in. (3–10 mm) 1/8 in. (3 mm) 2T
- 3/8 in. ≤ T < 1 in. (10–25 mm) 1/8 in. (3 mm) 2T
- T ≥ 1 in. (25 mm) 1/8 in. (3 mm) UNLIMITED (T = ∞)
Important
A test coupon welded on plate 1 in. (25 mm) thick or greater qualifies the WPS for all structural thicknesses from 1/8 in. (3 mm) to Unlimited . This is why the 1 in. plate test coupon is the industry standard for commercial procedure qualification programs.