15.2 Heat Treatment of Metals

Red Seal Industrial Mechanic Millwright

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: Safety & Occupational Skills

1.1 WHMIS, SDS & Hazardous Materials 1.2 Lockout/Tagout (LOTO) & Energy Isolation 1.3 Confined Space Entry & Fall Protection 1.4 Blueprint Reading, Trade Math & Precision Measurement Tools 1.5 Hand Tools, Portable Power Tools & Shop Machines 1.6 Access Equipment: Ladders, Scaffolds & Elevating Work Platforms 1.7 Planning Work, Permits, Communication & Mentoring

2 Chapter 2: Fasteners & Bolted Joints

2.1 Threaded Fasteners, Bolts & Thread Standards 2.2 Torque Values, Tightening Patterns & Thread Pitch/Gaging 2.3 Non-Threaded Fasteners, Pins, Keys & Anchors

3 Chapter 3: Rigging, Hoisting & Crane Signals

3.1 Sling Angles, Sling Types & Leg Tension Calculations 3.2 Working Load Limit (WLL) & Hardware Inspection 3.3 Centre of Gravity & Load Weight Estimation 3.4 Hoists, Overhead Cranes & Standard Hand Signals 3.5 Jacking, Skidding, Rollers & Moving Equipment 3.6 Lift Planning, Area Control & Rigging Equipment Maintenance

4 Chapter 4: Prime Movers & Electric Motors

4.1 Electric Motors, Enclosures, Frame Sizes & Synchronous Speed 4.2 Motor Installation, Nameplates & Overload Protection 4.3 Engine Prime Movers & Mechanical Drives Introduction

5 Chapter 5: Belt & Chain Mechanical Drives

5.1 V-Belts, Timing Belts & Sheave Alignment 5.2 Belt Tensioning, Pitch Diameter & Speed Ratios 5.3 Roller Chains, Sprocket Alignment & Lubrication 5.4 Clutches, Brakes & Torque Limiters

6 Chapter 6: Gear Drives, Couplings & Reducers

6.1 Gear Types, Geometry & Gear Ratios 6.2 Couplings (Rigid, Flexible, Fluid) & Installation 6.3 Shaft Keys, Keyways, Taper Sleeves & Hub Fits 6.4 Gear Reducers, Backlash & Mechanical Drive Troubleshooting

7 Chapter 7: Industrial Pumps & Systems

7.1 Centrifugal Pumps, Impellers & Performance Curves 7.2 Positive Displacement Pumps (Gear, Vane, Piston, Diaphragm) 7.3 Cavitation, NPSHa vs NPSHr & Pump Priming 7.4 Pump Maintenance, Packing & Mechanical Seals

8 Chapter 8: Compressors, Fans & Pneumatics

8.1 Reciprocating & Rotary Screw Air Compressors 8.2 Compressed Air Treatment, FRL Units & Air Receivers 8.3 Centrifugal & Axial Fans, Affinity Laws & Airflow 8.4 Pneumatic Circuits, Valves, Actuators & Troubleshooting 8.5 Vacuum Systems, Pumps & Venturi Generators

9 Chapter 9: Bearings, Lubrication & Seals

9.1 Plain Bearings, Bushings & Fits 9.2 Rolling Element Bearings & Installation 9.3 Bearing Heating Limits, Fits & Removal Tools 9.4 Industrial Lubricants, Viscosity, Grease NLGI Grades & Seals

10 Chapter 10: Precision Alignment & Foundations

10.1 Precision Shaft Alignment (Rim-and-Face & Reverse-Dial Methods) 10.2 Laser Alignment, Soft Foot Correction & Thermal Growth 10.3 Machinery Foundations, Leveling, Grouting & Dowelling

11 Chapter 11: Vibration Analysis & Predictive Maintenance

11.1 Vibration Analysis, Dynamic Balancing & Thermography 11.2 Preventive/Predictive Maintenance & Decommissioning 11.3 Non-Destructive Testing (NDT) Methods 11.4 Lubricant & Fluid Analysis 11.5 Commissioning: Pre-Start Checks, Run-In & Documentation

12 Chapter 12: Hydraulic Systems

12.1 Hydraulic Fundamentals: Pascal’s Law, Pressure, Flow & Power 12.2 Hydraulic Fluids, Reservoirs, Filtration & Contamination Control 12.3 Hydraulic Pumps: Gear, Vane & Piston Designs 12.4 Hydraulic Valves: Pressure, Directional & Flow Control 12.5 Hydraulic Actuators: Cylinders, Motors & Accumulators 12.6 Hydraulic Conductors, ISO 1219 Symbols & System Troubleshooting

13 Chapter 13: Conveying Systems, Material Handling & Automation

13.1 Belt Conveyors: Components, Tracking & Training 13.2 Screw, Bucket, Roller, Chain & Pneumatic Conveyors 13.3 Robotics & Automated Equipment

14 Chapter 14: Process Piping, Tanks & Vessels

14.1 Process Piping: Materials, Sizing, Fittings & Joining 14.2 Flanges, Gaskets & Piping Bolted-Joint Assembly 14.3 Tanks, Vessels & Containers: Installation, Inspection & Repair

15 Chapter 15: Materials, Fabrication, Cutting & Welding

15.1 Material Identification: Ferrous & Non-Ferrous Metals, Plastics 15.2 Heat Treatment of Metals 15.3 Oxy-Fuel & Plasma Arc Cutting 15.4 Welding Processes: SMAW, GMAW, GTAW, OFW & Equipment Care 15.5 Layout Procedures & Maintaining Precision Measuring Tools

15.2 Heat Treatment of Metals

Key Takeaways Explain This Topic AI

Annealing heats above the upper critical temperature then cools slowly in the furnace to give the softest, most ductile and most machinable condition.

Normalizing uses the same heating range but cools in still air, producing a finer, more uniform grain and higher strength than annealing.

Quenching forms hard, brittle martensite, and tempering below the lower critical temperature of 727 C then restores toughness at some cost in hardness.

Temper colours give a field indication of temperature: pale straw at about 220 C, brown-purple near 275 C and dark blue near 300 C.

Case hardening adds a hard surface to a low-carbon core — carburizing at 900–950 C requires a quench, while nitriding at 500–550 C hardens without quenching or distortion.

Last updated: August 2026

Sub-task A-3.07 (Performs heat treatment of metal) covers what a millwright does at the bench and in the field: annealing a work-hardened part before forming, normalizing after welding, hardening and tempering a punch or wear part, stress-relieving a fabrication, and specifying preheat for welding.

Critical Temperatures

Steel changes crystal structure as it is heated. Two temperatures matter:

Lower critical temperature (A1) = 727 C — the point at which pearlite begins to transform to austenite. All hardening treatments must exceed it; all tempering and stress relieving must stay below it.

Upper critical temperature (A3) — the point at which the steel is fully austenitic. It varies with carbon content, from about 900 C at 0.20% carbon down to 727 C at the 0.83% eutectoid composition.

For hardening and annealing, steel is heated roughly 30–50 C above the upper critical temperature , soaked long enough for the section to reach temperature throughout (a common rule is one hour per 25 mm of thickness), and then cooled at a rate that determines the result.

The Four Core Processes

Process Heat to Cooling rate Result

Annealing (full) Above upper critical Very slow — in the furnace Softest, most ductile, most machinable; relieves all stress; coarsens grain

Normalizing Above upper critical Still air Fine uniform grain, higher strength and toughness than annealed; standard after forging or heavy welding

Hardening Above upper critical Rapid quench Martensite: maximum hardness, very brittle, high internal stress

Tempering Below lower critical (150–650 C) Air Reduces brittleness and internal stress, increases toughness, lowers hardness slightly

Stress relieving is a fifth, separate treatment: heat to roughly 550–650 C (well below A1), soak, then cool slowly. It relaxes residual stress from welding, machining or cold work without changing the microstructure or hardness. It is what a millwright specifies for a welded frame that must hold alignment.

The hardening rule: only steels with more than about 0.30% carbon harden appreciably by quenching. Mild steel heated cherry red and dropped in water will not get hard, because there is not enough carbon to form significant martensite. A part that must be hard on the outside and tough in the core is case hardened instead.

Quench Media

Quench severity determines whether the part hardens fully — and whether it cracks or distorts.

  • Medium Severity Notes
  • Brine (salt water) Most severe Fastest; highest risk of quench cracking and distortion
  • Water Severe Plain carbon steels; agitate to break the vapour blanket
  • Polymer solution Adjustable Concentration sets the cooling rate between water and oil
  • Oil Moderate Alloy steels such as 4140; oil must be at the specified temperature, typically 50–65 C
  • Air / still air Mild Air-hardening tool steels (A-series), normalizing
  • Molten salt Controlled Martempering and austempering

Parts are quenched vertically, with the longest axis down and agitated , so cooling is even. Quenching a long shaft horizontally cools one side first and bows it permanently. A vapour blanket clinging to a surface causes soft spots, which is why agitation matters.

Tempering and Temper Colours

After quenching, a part is at maximum hardness and maximum brittleness, with high residual stress. It must be tempered promptly — a hardened part left overnight can crack on the shelf.

Tempering temperature sets the balance. On a clean polished surface, the oxide film colour gives a usable field indication:

  • Colour Approximate temperature Typical application
  • Pale / light straw 220 C Scrapers, lathe tools, hard punches
  • Dark straw 240 C Drills, taps, dies
  • Brown 255 C Cold chisels for hard material
  • Purple 275 C Centre punches, scribers
  • Dark blue 300 C Cold chisels, screwdrivers, springs needing toughness
  • Light blue / grey-blue 320–340 C Wood saws, springs

Higher tempering temperatures (400–650 C) are used on alloy steels such as 4140 to reach a specified hardness band like 28–32 HRC for a shaft. Note that some alloy steels suffer temper embrittlement if held in the 375–575 C range, so the manufacturer's tempering specification must be followed rather than a colour chart.

Case Hardening

Case hardening produces a hard, wear-resistant surface over a tough, shock-absorbing low-carbon core — exactly what a gear tooth, a pin or a cam follower needs.

Method Temperature Mechanism Notes

Carburizing 900–950 C Carbon diffuses into the surface from a gas, pack or salt medium Requires a quench and temper after ; case depth 0.5–2.5 mm; heavy distortion risk

Carbonitriding 800–900 C Carbon plus nitrogen Thinner case, less distortion than carburizing

Nitriding 500–550 C Nitrogen diffuses in, forming hard nitrides No quench required , minimal distortion, very hard case (up to about 70 HRC); needs a nitriding-grade alloy steel

Flame hardening Localized above upper critical Oxy-fuel torch then quench Selective hardening of gear teeth, ways, sprocket rims in the field

Induction hardening Localized above upper critical Induction coil then quench Fast, repeatable, minimal distortion; shaft journals, crankshafts

Nitriding is the low-distortion choice because it runs below the lower critical temperature, so no phase change and no quench occur. That is exactly why a precision component already ground to size can be nitrided but not carburized.

Heat Treatment of Non-Ferrous Metals

Copper, brass and aluminum behave differently, and confusing them with steel is a common error.

Copper and brass are annealed by heating to a dull red and then either quenching in water or air cooling. Unlike steel, quenching does not harden them — copper alloys have no hardening phase transformation. They harden only by work hardening (cold forming), and heating removes it.

Aluminum alloys in the heat-treatable series (2xxx, 6xxx, 7xxx) are solution treated, quenched, and then aged to a -T4 or -T6 temper. Overheating a T6 part with a torch annealsit locally and permanently destroys the temper — a fact that matters when a millwright straightens or welds aluminum guarding or structure.

Welding, Preheat and Post-Weld Heat Treatment

Heat treatment and welding meet in the heat-affected zone (HAZ) . Welding is a localized quench: molten metal against a cold mass cools fast enough to form brittle martensite in medium- and high-carbon steel, and hydrogen from moisture then drives hydrogen-induced (cold) cracking , which can appear up to 48 hours after welding.

Carbon equivalent (CE) predicts the risk: C E = C + M n 6 + C r + M o + V 5 + N i + C u 15 CE = C + \frac{Mn}{6} + \frac{Cr + Mo + V}{5} + \frac{Ni + Cu}{15} CE = C + 6 M n ​ + 5 C r + M o + V ​ + 15 N i + C u ​

  • CE value Weldability
  • Under 0.40 Readily weldable, generally no preheat
  • 0.40–0.45 Preheat advisable, especially on thick sections
  • 0.45–0.60 Preheat required , low-hydrogen consumables, controlled interpass temperature
  • Over 0.60 Preheat plus post-weld heat treatment; specialist procedure

Preheat slows the cooling rate, lets hydrogen diffuse out, and reduces shrinkage stress. It is applied to the whole joint region, not just the weld line, and interpass temperature is maintained through the weld. Post-weld heat treatment (PWHT) — typically a 595–675 C stress relief — is applied to thick, restrained or code-governed weldments.

Welding cast iron is a special case: preheat to about 260–320 C, weld with nickel-based electrodes (ENi-CI or ENiFe-CI) in short stringer beads, peen each bead while hot to relieve shrinkage, and cool very slowly under insulating blankets. Skipping the slow cool cracks the casting alongside the weld every time.

Field Safety

Heat-treating creates severe burn and fire hazards. Use dry tongs, face shield, leather gloves and apron, and keep quench tanks away from combustibles.

Never quench in a container of oil that has water in the bottom — the water flashes to steam and can throw burning oil.

Galvanized coating vapourizes near 900 C, producing zinc oxide fume and metal fume fever . Remove the coating and ventilate.

Hardened parts can shatter. Wear eye protection when striking, cutting or grinding a hardened component.