Study guide
15.1 Material Identification: Ferrous & Non-Ferrous Metals, Plastics
Red Seal Industrial Mechanic Millwright
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Safety & Occupational Skills
1.1 WHMIS, SDS & Hazardous Materials 1.2 Lockout/Tagout (LOTO) & Energy Isolation 1.3 Confined Space Entry & Fall Protection 1.4 Blueprint Reading, Trade Math & Precision Measurement Tools 1.5 Hand Tools, Portable Power Tools & Shop Machines 1.6 Access Equipment: Ladders, Scaffolds & Elevating Work Platforms 1.7 Planning Work, Permits, Communication & Mentoring
2 Chapter 2: Fasteners & Bolted Joints
2.1 Threaded Fasteners, Bolts & Thread Standards 2.2 Torque Values, Tightening Patterns & Thread Pitch/Gaging 2.3 Non-Threaded Fasteners, Pins, Keys & Anchors
3 Chapter 3: Rigging, Hoisting & Crane Signals
3.1 Sling Angles, Sling Types & Leg Tension Calculations 3.2 Working Load Limit (WLL) & Hardware Inspection 3.3 Centre of Gravity & Load Weight Estimation 3.4 Hoists, Overhead Cranes & Standard Hand Signals 3.5 Jacking, Skidding, Rollers & Moving Equipment 3.6 Lift Planning, Area Control & Rigging Equipment Maintenance
4 Chapter 4: Prime Movers & Electric Motors
4.1 Electric Motors, Enclosures, Frame Sizes & Synchronous Speed 4.2 Motor Installation, Nameplates & Overload Protection 4.3 Engine Prime Movers & Mechanical Drives Introduction
5 Chapter 5: Belt & Chain Mechanical Drives
5.1 V-Belts, Timing Belts & Sheave Alignment 5.2 Belt Tensioning, Pitch Diameter & Speed Ratios 5.3 Roller Chains, Sprocket Alignment & Lubrication 5.4 Clutches, Brakes & Torque Limiters
6 Chapter 6: Gear Drives, Couplings & Reducers
6.1 Gear Types, Geometry & Gear Ratios 6.2 Couplings (Rigid, Flexible, Fluid) & Installation 6.3 Shaft Keys, Keyways, Taper Sleeves & Hub Fits 6.4 Gear Reducers, Backlash & Mechanical Drive Troubleshooting
7 Chapter 7: Industrial Pumps & Systems
7.1 Centrifugal Pumps, Impellers & Performance Curves 7.2 Positive Displacement Pumps (Gear, Vane, Piston, Diaphragm) 7.3 Cavitation, NPSHa vs NPSHr & Pump Priming 7.4 Pump Maintenance, Packing & Mechanical Seals
8 Chapter 8: Compressors, Fans & Pneumatics
8.1 Reciprocating & Rotary Screw Air Compressors 8.2 Compressed Air Treatment, FRL Units & Air Receivers 8.3 Centrifugal & Axial Fans, Affinity Laws & Airflow 8.4 Pneumatic Circuits, Valves, Actuators & Troubleshooting 8.5 Vacuum Systems, Pumps & Venturi Generators
9 Chapter 9: Bearings, Lubrication & Seals
9.1 Plain Bearings, Bushings & Fits 9.2 Rolling Element Bearings & Installation 9.3 Bearing Heating Limits, Fits & Removal Tools 9.4 Industrial Lubricants, Viscosity, Grease NLGI Grades & Seals
10 Chapter 10: Precision Alignment & Foundations
10.1 Precision Shaft Alignment (Rim-and-Face & Reverse-Dial Methods) 10.2 Laser Alignment, Soft Foot Correction & Thermal Growth 10.3 Machinery Foundations, Leveling, Grouting & Dowelling
11 Chapter 11: Vibration Analysis & Predictive Maintenance
11.1 Vibration Analysis, Dynamic Balancing & Thermography 11.2 Preventive/Predictive Maintenance & Decommissioning 11.3 Non-Destructive Testing (NDT) Methods 11.4 Lubricant & Fluid Analysis 11.5 Commissioning: Pre-Start Checks, Run-In & Documentation
12 Chapter 12: Hydraulic Systems
12.1 Hydraulic Fundamentals: Pascal’s Law, Pressure, Flow & Power 12.2 Hydraulic Fluids, Reservoirs, Filtration & Contamination Control 12.3 Hydraulic Pumps: Gear, Vane & Piston Designs 12.4 Hydraulic Valves: Pressure, Directional & Flow Control 12.5 Hydraulic Actuators: Cylinders, Motors & Accumulators 12.6 Hydraulic Conductors, ISO 1219 Symbols & System Troubleshooting
13 Chapter 13: Conveying Systems, Material Handling & Automation
13.1 Belt Conveyors: Components, Tracking & Training 13.2 Screw, Bucket, Roller, Chain & Pneumatic Conveyors 13.3 Robotics & Automated Equipment
14 Chapter 14: Process Piping, Tanks & Vessels
14.1 Process Piping: Materials, Sizing, Fittings & Joining 14.2 Flanges, Gaskets & Piping Bolted-Joint Assembly 14.3 Tanks, Vessels & Containers: Installation, Inspection & Repair
15 Chapter 15: Materials, Fabrication, Cutting & Welding
15.1 Material Identification: Ferrous & Non-Ferrous Metals, Plastics 15.2 Heat Treatment of Metals 15.3 Oxy-Fuel & Plasma Arc Cutting 15.4 Welding Processes: SMAW, GMAW, GTAW, OFW & Equipment Care 15.5 Layout Procedures & Maintaining Precision Measuring Tools
15.1 Material Identification: Ferrous & Non-Ferrous Metals, Plastics
Key Takeaways Explain This Topic AI
In the AISI/SAE four-digit system the last two digits give carbon content in hundredths of a percent, so 1045 is a plain carbon steel with 0.45% carbon and 4140 is a chrome-moly steel with 0.40% carbon.
Austenitic 300-series stainless steel is non-magnetic in the annealed condition, while ferritic and martensitic 400-series stainless steels are magnetic — the fastest field discriminator.
Only steels above roughly 0.30% carbon will harden appreciably by quenching, which is why low-carbon structural steel cannot be hardened but can be case hardened.
Spark testing reads carbon content: low-carbon steel throws long straw streaks with few forks, high-carbon steel throws dense repeating bursts, and cast iron throws short dull red streaks.
Positive material identification with a portable X-ray fluorescence analyzer is the only definitive field method for alloy verification on code work.
Last updated: August 2026
Sub-task A-3.06 (Performs material identification) sits inside Task A-3, which carries 7 of the 25 questions in Major Work Activity A. Selecting the wrong material for a shaft, a wear plate or a repair weld is a failure that shows up weeks later, so the exam tests whether a journeyperson can classify what is in front of them.
The AISI / SAE Numbering System
Plain carbon and alloy steels use a four-digit designation:
Digits Meaning
First digit Major alloy family — 1 carbon, 2 nickel, 3 nickel-chromium, 4 molybdenum, 5 chromium, 6 chromium-vanadium, 8 nickel-chrome-moly, 9 silicon-manganese
- Second digit Approximate percentage of the principal alloying element, or a sub-class
- Last two digits Carbon content in hundredths of one percent
- Grade Reads as Typical millwright use
- 1018 Plain carbon, 0.18% C General shafting, machine parts, weldable, case-hardens well
- 1045 Plain carbon, 0.45% C Medium-carbon shafting, keys, gears; through-hardenable
- 4140 Chrome-moly, 0.40% C High-strength shafts, bolts, hydraulic rams — the workhorse alloy steel
- 4340 Ni-Cr-Mo, 0.40% C Heavily loaded shafts and gears
- 8620 Ni-Cr-Mo, 0.20% C Carburizing grade for gears and pins
- 52100 High-carbon chromium, 1.00% C Rolling-element bearing steel (also called 100Cr6)
- Carbon Ranges and Their Consequence
Class Carbon Behaviour
Low carbon (mild) Under 0.30% Readily welded and formed; does not harden appreciably by quenching ; case-harden instead
- Medium carbon 0.30–0.60% Through-hardenable; needs preheat for welding above about 0.35%
- High carbon 0.60–1.00% Springs, cutting edges, wear parts; difficult to weld, high cracking risk
- Tool steel 0.70%+ with alloys Water-hardening (W), oil-hardening (O), air-hardening (A), high-speed (M, T)
The rule that follows is worth memorizing: weldability falls and hardenability rises as carbon content rises. A shaft that hardens under a torch flame is a medium- or high-carbon steel, and welding it without preheat will crack it.
Cast Irons
Type Structure Characteristics
Grey cast iron Graphite flakes Excellent damping and machinability; brittle in tension; machine bases, housings, pump casings
Ductile (nodular) iron Spheroidal graphite Much higher tensile strength and impact resistance; crankshafts, gears, valve bodies
- White cast iron Cementite, no free graphite Extremely hard and abrasion resistant; unmachinable; wear liners
- Malleable iron Heat-treated white iron Ductile and shock resistant; pipe fittings, brackets
Grey iron is identified by a dull grey fracture face that leaves a grey mark on your hand from the graphite, whereas steel fractures bright.
Stainless Steels
Family Series Magnetic? Notes
Austenitic 300 (304, 316, 321) Non-magnetic when annealed (can become slightly magnetic after cold work) Cannot be hardened by heat treatment, only by cold work; 316 adds molybdenum for chloride resistance
- Ferritic 400 (409, 430) Magnetic Moderate corrosion resistance; not hardenable by quenching
- Martensitic 400 (410, 416, 420, 440) Magnetic Hardenable by quench and temper ; shafts, valve stems, cutlery
- Duplex 2205, 2507 Magnetic Austenite plus ferrite; high strength and chloride-stress-corrosion resistance
- Precipitation hardening 17-4 PH Magnetic Very high strength; pump and valve shafts
The magnet is the fastest field test: a shaft that a magnet will not stick to, in a corrosive service, is almost certainly 304 or 316. That matters immediately because austenitic grades cannot be hardened by heat treatment and are prone to galling on threads unless anti-seize is used.
Non-Ferrous Metals and Bearing Alloys
Metal Identification Use
Aluminum Light (about one third the weight of steel), non-magnetic, grey oxide Guards, light structures; 6061-T6 is the general machining grade
- Copper Reddish, very high conductivity Electrical, tubing, gaskets
- Brass (Cu-Zn) Yellow Fittings, bushings, valve internals
- Bronze (Cu-Sn) Reddish-brown; harder than brass Sleeve bearings, wear plates, worm gears
Babbitt (tin or lead based) Very soft, silver Poured or lined plain bearings; embeds dirt and protects the shaft
- Monel (Ni-Cu) Grey, non-magnetic to weakly magnetic, very tough Seawater and chemical service
- Titanium Very light, extremely tough, sparks bright white Chemical process, aggressive corrosion
Aluminum temper designations appear constantly on machine parts: -O annealed, -Hxx strain hardened (non-heat-treatable alloys), -T4 solution treated and naturally aged, -T6 solution treated and artificially aged (the common structural condition).
Engineering Plastics and Composites
Millwrights increasingly install plastic wear components, chain guides and bearings.
Material Key property Typical application
UHMW-PE Extremely low friction, high abrasion resistance, self-lubricating Chain guides, wear strips, chute liners, star wheels
Nylon (PA) Tough, absorbs moisture and swells Sheaves, bushings, gears
Acetal (POM / Delrin) Dimensionally stable, low moisture absorption, machines cleanly Precision bushings and gears
- PTFE Lowest friction, chemically inert, poor creep resistance Seals, non-stick surfaces, chemical service
- PEEK High temperature (to about 250 C), high strength Demanding bearings and seals
- HDPE Chemically resistant, weldable Tanks, piping, liners
- Fibreglass (FRP) Corrosion resistant, non-conductive Gratings, tanks, ducting
Plastic bearing selection trap: nylon absorbs moisture and can swell by 2–3%, so a nylon bushing machined to a tight clearance in a dry shop will seize once it is wet. Acetal or UHMW is used where dimensional stability matters.
Field Identification Tests
Test Method What it tells you
Magnet Touch a magnet to a clean surface Separates austenitic stainless (non-magnetic) from carbon and 400-series steel (magnetic)
- Spark Touch to a grinding wheel in a darkened area and read the stream Carbon content and alloy family
- File Draw a sharp file across an edge Soft material cuts easily; hardened material skates and will not cut
Chip Cut a chip with a cold chisel Ductile materials give a continuous curl; cast iron gives short brittle chips
- Appearance and weight Colour, oxide, density Distinguishes aluminum, copper alloys, and cast iron
- Sound (ring test) Suspend and strike A cracked casting or roll gives a dull thud instead of a ring
- Hardness test Rockwell, Brinell, or portable hardness tester Confirms heat-treated condition
PMI / portable XRF X-ray fluorescence analyzer The only definitive field alloy verification ; required on code piping and pressure work
- Reading a Spark Test WROUGHT IRON Long straight straw-yellow streaks, forked ends, no bursts
- LOW-CARBON STEEL Long straw streaks with a few small forks near the end
- MEDIUM CARBON More numerous forks and small starbursts along the stream
- HIGH-CARBON STEEL Dense, bright, repeating multi-branch bursts near the wheel
- CAST IRON Short, dull RED streaks that brighten and burst near the end
- STAINLESS (300) Short, straw-coloured stream, few forks, less brilliant
- HIGH-SPEED STEEL Faint dark red stream with distinctive orange spear points
Spark testing is a comparison method: keep known reference samples at the grinder and compare. It gives a family, not a grade.
Mechanical Properties the Exam Uses
- Property Definition Practical meaning
- Tensile strength Maximum stress before fracture Ultimate capacity of a shaft or bolt
Yield strength Stress at which permanent deformation begins The real design limit — a bolt stretched past yield loses preload
- Ductility Elongation percentage before fracture Ability to deform rather than snap
- Hardness Resistance to indentation Correlates with wear resistance and tensile strength in steel
- Toughness Energy absorbed before fracture (Charpy impact) Resistance to shock, especially at low temperature
Fatigue strength Stress a part survives for a set number of cycles Governs rotating shafts; a sharp corner or keyway is a fatigue initiator
Hardness scales: Rockwell C (HRC) for hardened steel above about 20 HRC, Rockwell B (HRB) for softer steels and non-ferrous, and Brinell (HB) for castings and large sections using a 10 mm ball at 3,000 kg. A shaft specified at 28–32 HRC is a quenched-and-tempered medium-carbon or alloy steel, not mild steel.
Low-temperature toughness is a Canadian issue. Ordinary carbon steel undergoes a ductile-to-brittle transition as temperature falls; structural and lifting components used outdoors in winter must be specified with notch-toughness requirements. Hoisting a load with a shackle or lifting lug made from an unrated steel at -30 C risks brittle fracture with no warning.