Study guide
15.4 Welding Processes: SMAW, GMAW, GTAW, OFW & Equipment Care
Red Seal Industrial Mechanic Millwright
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Safety & Occupational Skills
1.1 WHMIS, SDS & Hazardous Materials 1.2 Lockout/Tagout (LOTO) & Energy Isolation 1.3 Confined Space Entry & Fall Protection 1.4 Blueprint Reading, Trade Math & Precision Measurement Tools 1.5 Hand Tools, Portable Power Tools & Shop Machines 1.6 Access Equipment: Ladders, Scaffolds & Elevating Work Platforms 1.7 Planning Work, Permits, Communication & Mentoring
2 Chapter 2: Fasteners & Bolted Joints
2.1 Threaded Fasteners, Bolts & Thread Standards 2.2 Torque Values, Tightening Patterns & Thread Pitch/Gaging 2.3 Non-Threaded Fasteners, Pins, Keys & Anchors
3 Chapter 3: Rigging, Hoisting & Crane Signals
3.1 Sling Angles, Sling Types & Leg Tension Calculations 3.2 Working Load Limit (WLL) & Hardware Inspection 3.3 Centre of Gravity & Load Weight Estimation 3.4 Hoists, Overhead Cranes & Standard Hand Signals 3.5 Jacking, Skidding, Rollers & Moving Equipment 3.6 Lift Planning, Area Control & Rigging Equipment Maintenance
4 Chapter 4: Prime Movers & Electric Motors
4.1 Electric Motors, Enclosures, Frame Sizes & Synchronous Speed 4.2 Motor Installation, Nameplates & Overload Protection 4.3 Engine Prime Movers & Mechanical Drives Introduction
5 Chapter 5: Belt & Chain Mechanical Drives
5.1 V-Belts, Timing Belts & Sheave Alignment 5.2 Belt Tensioning, Pitch Diameter & Speed Ratios 5.3 Roller Chains, Sprocket Alignment & Lubrication 5.4 Clutches, Brakes & Torque Limiters
6 Chapter 6: Gear Drives, Couplings & Reducers
6.1 Gear Types, Geometry & Gear Ratios 6.2 Couplings (Rigid, Flexible, Fluid) & Installation 6.3 Shaft Keys, Keyways, Taper Sleeves & Hub Fits 6.4 Gear Reducers, Backlash & Mechanical Drive Troubleshooting
7 Chapter 7: Industrial Pumps & Systems
7.1 Centrifugal Pumps, Impellers & Performance Curves 7.2 Positive Displacement Pumps (Gear, Vane, Piston, Diaphragm) 7.3 Cavitation, NPSHa vs NPSHr & Pump Priming 7.4 Pump Maintenance, Packing & Mechanical Seals
8 Chapter 8: Compressors, Fans & Pneumatics
8.1 Reciprocating & Rotary Screw Air Compressors 8.2 Compressed Air Treatment, FRL Units & Air Receivers 8.3 Centrifugal & Axial Fans, Affinity Laws & Airflow 8.4 Pneumatic Circuits, Valves, Actuators & Troubleshooting 8.5 Vacuum Systems, Pumps & Venturi Generators
9 Chapter 9: Bearings, Lubrication & Seals
9.1 Plain Bearings, Bushings & Fits 9.2 Rolling Element Bearings & Installation 9.3 Bearing Heating Limits, Fits & Removal Tools 9.4 Industrial Lubricants, Viscosity, Grease NLGI Grades & Seals
10 Chapter 10: Precision Alignment & Foundations
10.1 Precision Shaft Alignment (Rim-and-Face & Reverse-Dial Methods) 10.2 Laser Alignment, Soft Foot Correction & Thermal Growth 10.3 Machinery Foundations, Leveling, Grouting & Dowelling
11 Chapter 11: Vibration Analysis & Predictive Maintenance
11.1 Vibration Analysis, Dynamic Balancing & Thermography 11.2 Preventive/Predictive Maintenance & Decommissioning 11.3 Non-Destructive Testing (NDT) Methods 11.4 Lubricant & Fluid Analysis 11.5 Commissioning: Pre-Start Checks, Run-In & Documentation
12 Chapter 12: Hydraulic Systems
12.1 Hydraulic Fundamentals: Pascal’s Law, Pressure, Flow & Power 12.2 Hydraulic Fluids, Reservoirs, Filtration & Contamination Control 12.3 Hydraulic Pumps: Gear, Vane & Piston Designs 12.4 Hydraulic Valves: Pressure, Directional & Flow Control 12.5 Hydraulic Actuators: Cylinders, Motors & Accumulators 12.6 Hydraulic Conductors, ISO 1219 Symbols & System Troubleshooting
13 Chapter 13: Conveying Systems, Material Handling & Automation
13.1 Belt Conveyors: Components, Tracking & Training 13.2 Screw, Bucket, Roller, Chain & Pneumatic Conveyors 13.3 Robotics & Automated Equipment
14 Chapter 14: Process Piping, Tanks & Vessels
14.1 Process Piping: Materials, Sizing, Fittings & Joining 14.2 Flanges, Gaskets & Piping Bolted-Joint Assembly 14.3 Tanks, Vessels & Containers: Installation, Inspection & Repair
15 Chapter 15: Materials, Fabrication, Cutting & Welding
15.1 Material Identification: Ferrous & Non-Ferrous Metals, Plastics 15.2 Heat Treatment of Metals 15.3 Oxy-Fuel & Plasma Arc Cutting 15.4 Welding Processes: SMAW, GMAW, GTAW, OFW & Equipment Care 15.5 Layout Procedures & Maintaining Precision Measuring Tools
15.4 Welding Processes: SMAW, GMAW, GTAW, OFW & Equipment Care
Key Takeaways Explain This Topic AI
In the AWS electrode classification E7018, the 70 means 70,000 psi tensile strength, the 1 means all positions, and the 8 identifies a low-hydrogen iron-powder coating.
E7018 low-hydrogen electrodes must be kept in a heated rod oven at roughly 120 C after the sealed container is opened, because absorbed moisture causes hydrogen cracking.
GMAW short-circuit transfer suits thin material and out-of-position work, while spray transfer requires higher current and argon-rich gas and is limited to flat and horizontal positions.
GTAW uses direct current electrode negative for steel and stainless, and alternating current for aluminum so the reverse-polarity half cycle breaks up the refractory oxide layer.
Cast iron repair welding requires 260–320 C preheat, nickel-based electrodes, short stringer beads peened while hot, and a very slow insulated cool-down.
Last updated: August 2026
Sub-tasks A-6.02 through A-6.06 cover joining and welding with oxy-fuel, SMAW, GMAW and GTAW equipment, plus maintaining that equipment. Millwrights are not welders by trade, but the interprovincial standard expects a journeyperson to perform routine welding competently, recognize defects, and know when a job requires a certified welder under a qualified procedure.
Process Comparison
Process Common name Electrode Shielding Best for
SMAW Stick Consumable, flux-coated Flux decomposition gas and slag Field repair, dirty or rusty steel, wind, all positions, heavy sections
GMAW MIG Consumable solid wire External gas (CO2, Ar/CO2, Ar/O2) Fast production welding indoors on clean steel
FCAW Flux core Consumable tubular wire Flux, with or without external gas High deposition; self-shielded FCAW-S works outdoors
GTAW TIG Non-consumable tungsten Argon or Ar/He Highest quality, thin material, stainless, aluminum, root passes
OFW Gas welding Filler rod Oxy-acetylene flame Thin steel, brazing, torch brazing of tubing; largely superseded
SMAW and AWS Electrode Classification
The AWS A5.1 code E XX Y Z is decoded left to right:
- Position Meaning Example: E7018
- E Electrode Electrode
- XX Tensile strength in thousands of psi 70 = 70,000 psi
- Y Welding positions 1 = all positions (2 = flat and horizontal fillet; 4 = includes vertical down)
- Z Coating type and current 8 = low-hydrogen, iron powder; AC or DCEP
- Electrode Character Millwright use
- E6010 Cellulose, DCEP, deep digging penetration, forceful arc Root passes on pipe, dirty or rusty steel
- E6011 E6010 chemistry runnable on AC Same as 6010 where only an AC machine is available
- E6013 Rutile, soft arc, shallow penetration, easy slag Sheet metal, light fabrication, poor fit-up
E7018 Low hydrogen , iron powder, smooth arc, high toughness Structural steel, high-carbon and alloy steels, code work
- ENi-CI / ENiFe-CI Nickel-based Cast iron repair
- E308L / E309L Stainless 308L for 300-series to itself; 309L for stainless to carbon steel (dissimilar joints)
Low-hydrogen storage is a hard rule. E7018 coatings absorb atmospheric moisture, and that moisture becomes hydrogen in the weld pool, driving delayed cracking in hardenable steels. Once a sealed container is opened, the electrodes go into a heated rod oven at about 120 C , and only the rods needed for the immediate task come out. Rods left out beyond the manufacturer's exposure limit must be re-conditioned or discarded.
Polarity conventions: DCEP (reverse polarity) puts about two thirds of the heat in the electrode, giving deeper penetration and better cleaning — the standard for E7018 and E6010. DCEN (straight polarity) puts more heat in the work, favouring faster melt-off on thin material and used for GTAW on steel.
GMAW: Gas and Transfer Mode
- Shielding gas Behaviour
- 100% CO2 Deepest penetration, cheapest, most spatter, short-circuit only
- 75% Ar / 25% CO2 The general-purpose mix: good penetration, low spatter, stable arc
- Ar with 1–5% O2 or 8% CO2 Enables spray transfer on carbon steel
- 100% Argon Aluminum and non-ferrous only
- Ar / He / CO2 tri-mix Stainless steel
Transfer mode Current Characteristics Position
Short circuit (dip) Low Wire touches the pool and short-circuits ~100 times per second; low heat input All positions , thin material
Globular Medium Large irregular droplets; high spatter; generally avoided Flat
Spray High, argon-rich gas Fine droplets propelled across the arc; high deposition, excellent fusion Flat and horizontal only — the pool is too fluid otherwise
Pulsed spray Pulsed Spray quality at a lower average heat All positions with the right equipment
The classic GMAW defect is cold lap / lack of fusion from short-circuit transfer used at too low a heat on thick material: the weld looks acceptable but has not fused to the base metal.
GTAW
GTAW uses a non-consumable tungsten electrode with filler added separately by hand.
DCEN for carbon steel, stainless, copper and titanium — maximum penetration, minimal tungsten heating.
AC for aluminum and magnesium . Aluminum carries a refractory oxide film melting near 2,050 C over metal melting near 660 C. The electrode-positive half cycle provides cathodic cleaning that breaks up that oxide, while the electrode-negative half cycle provides penetration.
High-frequency start avoids contaminating the tungsten by scratch-starting.
Tungsten types: 2% thoriated (red — mildly radioactive, avoid grinding dust), 2% lanthanated (blue) and 2% ceriated (grey) are the common non-radioactive substitutes, and pure tungsten (green) for AC on older machines.
Grind the tungsten longitudinally , with the grinding marks running along the electrode axis, so the arc stays stable.
Joints, Weld Types and Positions
Five basic joints: butt, lap, tee, corner, edge.
Weld types: fillet (triangular, at a tee or lap), groove (square, V, bevel, U, J), plug and slot, surfacing (hardfacing).
Positions are examined constantly:
- Code Plate Pipe
- 1F / 1G Flat Pipe rotated, welded at the top
- 2F / 2G Horizontal Pipe vertical, weld horizontal
- 3F / 3G Vertical —
- 4F / 4G Overhead —
- 5G — Pipe horizontal and fixed , welder moves around it
- 6G — Pipe fixed at 45 degrees — the all-position qualification test
F denotes a fillet weld and G a groove weld. Qualifying on 6G qualifies a welder for essentially all positions, which is why it is the benchmark pipe test.
Weld Defects and Their Causes
Defect Appearance Principal causes
Undercut Groove melted into the base metal at the toe, not filled Excessive current, too long an arc, wrong angle, too fast a travel speed
Porosity Gas holes in the weld Moisture, oil, paint, rust, galvanizing; lost shielding gas from wind or a blocked nozzle
Slag inclusion Trapped non-metallic material Poor interpass cleaning, wrong electrode angle, too low current
Lack of fusion / cold lap Weld metal not bonded to base metal Heat input too low, dirty surface, incorrect technique
Incomplete penetration Root of the joint not reached Root opening too small, land too thick, current too low, travel too fast
Cracks — hot In the weld while solidifying High sulphur or phosphorus, deep narrow bead, high restraint
Cracks — cold (hydrogen) In the HAZ, delayed hours to days Hydrogen from moisture, fast cooling, hardenable steel, no preheat
Overlap Weld metal rolled over the base without fusing Too slow travel, too low current
Arc strike A stray melted spot outside the weld Careless electrode contact; a fatigue crack initiator that must be ground out and inspected
- Distortion Warping, angular change, shrinkage Uncontrolled heat input and sequence
- Controlling Distortion
Weld metal shrinks as it cools, and that shrinkage bends the work. Standard controls:
Tack weld with adequate size and spacing, and use tacks that will be consumed or ground.
Back-step welding — weld short segments in the direction opposite to overall progression.
Skip / intermittent welding — distribute heat rather than laying one continuous pass.
Balanced welding — alternate sides of a joint or member so shrinkage forces oppose.
Pre-setting / pre-bending the parts so shrinkage pulls them into alignment.
Fixturing and strongbacks to restrain the work — but recognize that restraint raises residual stress and cracking risk in hardenable steel.
Minimum heat input — the smallest bead that meets the specification, with controlled interpass temperature.
Welding Equipment Maintenance (A-6.06)
Equipment Checks
Welding machine Clean cooling air passages; check fan operation; inspect the primary cord, plug and disconnect; verify the case ground
Cables and connections Look for cuts, exposed conductor, hot or discoloured lugs; a loose work-clamp connection causes arc instability, low voltage at the arc and overheating
Work (ground) clamp Clean bare metal contact, close to the weld; never route the return through bearings, gearboxes or rolling elements — arc current through a bearing causes electrical fluting damage
Electrode holder / gun Insulation intact, jaws clean; replace a cracked holder
GMAW gun consumables Contact tip sized to the wire and replaced when worn oval; nozzle cleaned of spatter and anti-spatter applied; liner matched to wire size and blown out or replaced — a worn liner is the leading cause of erratic wire feed
Drive rolls Groove matched to wire size and type (V for solid, knurled for flux-cored); tension set to the minimum that stops slipping
Shielding gas train Regulator and flowmeter accuracy; leak-test hoses and connections with soap solution; check flow at the nozzle, not just the flowmeter
- Rod oven Verify actual temperature with a thermometer, not just the dial
- Special Case: Welding Cast Iron
Clean the area and drill stop holes at the ends of the crack to prevent it running.
Vee out the crack, removing all the graphite-contaminated metal.
Preheat to 260–320 C slowly and uniformly.
Weld with nickel electrodes (ENi-CI or ENiFe-CI) using short stringer beads about 25–50 mm long , not long continuous runs.
Peen each bead while hot to relieve shrinkage stress.
Allow the casting to cool very slowly , buried in lime or wrapped in insulating blankets. A fast cool cracks the casting beside the weld every time.
Welding Safety
Fume: stainless steel produces hexavalent chromium , a confirmed carcinogen with a very low exposure limit; manganese fume is a neurotoxin; galvanized coating produces zinc oxide fume and metal fume fever. Local exhaust ventilation at the arc, or an air-supplied respirator, is required — not just a fan.
Arc radiation: ultraviolet light causes arc eye and skin burns within minutes. Use the correct shade, cover all skin, and screen the area to protect others.
Electric shock: open-circuit voltage is dangerous, especially when a welder is sweating or working in a damp confined space. Never drape cables over the body; keep dry gloves and dry insulation underfoot.
Fire: hot work permit, cleared and protected combustibles, and a fire watch for at least 30 minutes after work ends.
Never weld on a sealed vessel or a container that has held flammables until it is cleaned, purged and tested. A sealed vessel can also explode from expanding trapped gas even if the contents were inert.