Study guide
10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation
Key Takeaways Explain This Topic AI
Isothermal Transformation (TTT) diagrams assume instantaneous quenching to a constant temperature, whereas Continuous Cooling Transformation (CCT) diagrams govern welding, where transformation start and finish curves are shifted to longer times and depressed to lower temperatures.
Weld metal solidification mode (planar, cellular, columnar dendritic, or equiaxed dendritic) is governed by the constitutional supercooling criterion G_L / R < ΔT_0 / D_L; as the solid-liquid interface moves from the fusion line toward the weld centerline, G_L decreases and R increases, promoting dendritic breakdown.
Solute redistribution during non-equilibrium solidification is quantified by the Scheil equation C_s = k C_0 (1 - f_s)^(k-1); elements with low partition coefficients (S, P) segregate intensely into the terminal interdendritic liquid, forming low-melting eutectic films that cause solidification cracking unless mitigated by Mn/S control.
Martensite forms via an athermal, diffusionless shear mechanism when the cooling rate exceeds the critical cooling velocity; its transformation start (Ms) and finish (Mf) temperatures are governed by carbon and substitutional alloy content per the Andrews equations.
Last updated: September 2026
10.2 Continuous Cooling Transformation (CCT) & Solidification Microstructures
Quick Answer: Welding is fundamentally a non-equilibrium process characterized by rapid, continuous cooling rather than isothermal holds. Consequently, Continuous Cooling Transformation (CCT) diagrams—not isothermal Time-Temperature-Transformation (TTT) diagrams—must be used to predict weld metal and HAZ microstructures. In CCT diagrams, transformation noses are shifted down in temperature and to longer times. Weld pool solidification morphology transitions from planar to cellular, columnar dendritic, and equiaxed dendritic per the constitutional supercooling criterion ( G L / R < Δ T 0 / D L G_L/R < \Delta T_0 / D_L G L / R < Δ T 0 / D L ). Solute segregation into terminal interdendritic liquid is modeled by the Scheil equation ( C s = k C 0 ( 1 − f s ) k − 1 C_s = k C_0 (1 - f_s)^{k-1} C s = k C 0 ( 1 − f s ) k − 1 ), explaining why sulfur and phosphorus ( k ≈ 0.05 k \approx 0.05 k ≈ 0.05 ) trigger hot cracking. For optimal low-temperature Charpy toughness, weld metals are formulated to promote intragranularly nucleated acicular ferrite (AF) over grain-boundary upper bainite. Martensite forms via diffusionless shear below the Martensite Start ( M s M_s M s ) temperature, calculated using Andrews empirical formulas.
TTT vs. CCT Diagrams: Non-Equilibrium Weld Cooling Kinetics
In furnace heat treatment, steel components can be rapidly quenched into a salt bath and held isothermally at a fixed temperature to generate specific microstructures (such as austempering to produce lower bainite). These transformations are mapped on Time-Temperature-Transformation (TTT) or Isothermal Transformation (IT) diagrams.
In fusion welding, however, molten and heated metal undergoes continuous, non-linear cooling driven by thermal conduction into the surrounding cold base plate. The microstructural evolution during this continuous descent must be analyzed using Continuous Cooling Transformation (CCT) diagrams. ISOTHERMAL (TTT) vs. CONTINUOUS COOLING (CCT)
- Temp ^ Temp ^
- | Ae3 | Ae3
- | ----- | -----
- | \ | \ Continuous Cooling Curves
- | \ | \ (Fast ---> Slow)
- | +-----\--+ | \ \ \ \
- | | TTT | | | \ \ \ \
- | | Nose| | | +-----\----+ \ \
- | +-----+--+ | | CCT | \ \ \
- | \ | | Nose| \ \ \
- | \ | +-----+-------+ \ \
- | Ms ----------- | Ms -------------------
- +------------------------> +------------------------>
- Time (log t) Time (log t)
TTT: Instantaneous quench to constant T CCT: Temperature continuously drops;
Holds isothermally. Noses shift DOWN and to the RIGHT.
The Thermodynamic & Kinetic Shift in CCT Diagrams
When comparing CCT diagrams to their parent TTT diagrams for an identical steel composition:
Shift to Longer Times (Rightward Displacement): During continuous cooling, steel spends finite time passing through elevated temperatures where the thermodynamic driving force (undercooling Δ T = T e − T \Delta T = T_e - T Δ T = T e − T ) is small. Nucleation incubation accumulates incrementally along the cooling path. Consequently, the apparent transformation "start" and "finish" boundaries are displaced to longer times .
Shift to Lower Temperatures (Downward Displacement): Because cooling is continuous, transformation does not complete at the high-temperature incubation point; latent heat is released while the material drops into lower temperature regimes. The transformation noses for ferrite, pearlite, and bainite are shifted downward by 20 ∘ C 20^\circ\text{C} 2 0 ∘ C to > 50 ∘ C >50^\circ\text{C} > 5 0 ∘ C relative to isothermal TTT noses.
Depression or Elimination of Intermediate Phases: Rapid continuous cooling curves can bypass the ferrite and pearlite transformation "noses" entirely. If the cooling rate exceeds the critical cooling velocity ( C R crit CR_{\text{crit}} C R crit ), diffusion is suppressed, and austenite transforms purely into non-equilibrium martensite.
The Cooling Parameter: Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5
In international welding engineering (EN ISO, IIW), cooling severity is quantified by Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 —the elapsed time in seconds required for the weld deposit or HAZ to cool from 800 ∘ C 800^\circ\text{C} 80 0 ∘ C to 500 ∘ C 500^\circ\text{C} 50 0 ∘ C . This temperature window represents the critical kinetic corridor where austenite decomposes into ferrite, pearlite, bainite, or martensite. Fast cooling (small Δ t 8 / 5 < 5 s \Delta t_{8/5} < 5\text{ s} Δ t 8/5 < 5 s , low heat input, thick plates) yields hard martensite/bainite; slow cooling (large Δ t 8 / 5 > 30 s \Delta t_{8/5} > 30\text{ s} Δ t 8/5 > 30 s , high heat input, high preheat) yields coarse ferrite and pearlite.
Weld Metal Solidification Dynamics & Constitutional Supercooling
Solidification in fusion welding occurs epitaxially from the partially melted grains at the fusion boundary. The solidifying interface morphology is dictated by the Constitutional Supercooling Criterion formulated by Tiller, Jackson, Rutter, and Chalmers. CONSTITUTIONAL SUPERCOOLING CRITERION
- Liquidus Temp ^ Concentration ^
- | Liquid C_L | Liquid
- | / | /--------
- T_L --+---/ Solidus | / Solute Boundary
- | / C_0 ----+-----/ Layer (δ_N)
- T_S --+-/ | /|
- +-------------------> | / | C_s = k*C_L
- Distance (x) +------------------->
- Distance (x)
- STABLE PLANAR FRONT (High G_L / R) DENDRITIC BREAKDOWN (Low G_L / R)
- Solid Liquid Solid Liquid
- +-------+ +-------+
- | | | | Columnar
- | |=======> Solidification | |===/\==/\==> Dendrites
- | | Front | | \/ \/
- +-------+ +-------+
- The Constitutional Supercooling Equation
During solidification of an alloy, solute is rejected into the liquid (for solutes with equilibrium partition coefficient k < 1 k < 1 k < 1 ). This creates a solute-enriched boundary layer ahead of the advancing solid interface, locally depressing the thermodynamic liquidus temperature ( T L T_L T L ). If the actual thermal gradient in the liquid ( G L G_L G L ) is shallower than the liquidus temperature gradient ( d T L / d x dT_L/dx d T L / d x ), a zone of constitutionally supercooled liquid exists ahead of the interface: G L R < Δ T 0 D L = m L C 0 ( 1 − k ) k D L \frac{G_L}{R} < \frac{\Delta T_0}{D_L} = \frac{m_L C_0 (1 - k)}{k D_L} R G L < D L Δ T 0 = k D L m L C 0 ( 1 − k )
where:
G L = d T d x G_L = \frac{dT}{dx} G L = d x d T : Thermal temperature gradient in the liquid at the interface ( K/mm \text{K/mm} K/mm or ∘ C/cm ^\circ\text{C/cm} ∘ C/cm ).
R R R : Solidification interface growth velocity ( mm/s \text{mm/s} mm/s ).
Δ T 0 = T liquidus − T solidus \Delta T_0 = T_{\text{liquidus}} - T_{\text{solidus}} Δ T 0 = T liquidus − T solidus : Equilibrium freezing temperature range ( ∘ C ^\circ\text{C} ∘ C ).
m L m_L m L : Slope of the equilibrium liquidus line ( ∘ C/wt % ^\circ\text{C/wt}\% ∘ C/wt % ).
C 0 C_0 C 0 : Nominal bulk alloy solute concentration ( wt % \text{wt}\% wt % ).
k = C S / C L k = C_S / C_L k = C S / C L : Equilibrium partition coefficient.
D L D_L D L : Diffusion coefficient of the solute in the liquid melt (typically ∼ 3 × 10 − 5 cm 2 /s \sim 3 \times 10^{-5}\text{ cm}^2\text{/s} ∼ 3 × 1 0 − 5 cm 2 /s ).
Morphological Transitions Across the Weld Pool
As the ratio G L / R G_L / R G L / R progressively decreases, the advancing solid-liquid interface becomes unstable, evolving through four distinct morphologies: Planar → decreasing G L / R Cellular → Columnar Dendritic → Equiaxed Dendritic \text{Planar} \xrightarrow{\text{decreasing } G_L/R} \text{Cellular} \xrightarrow{} \text{Columnar Dendritic} \xrightarrow{} \text{Equiaxed Dendritic} Planar decreasing G L / R Cellular Columnar Dendritic Equiaxed Dendritic
In a moving weld pool, the local solidification velocity R R R and thermal gradient G L G_L G L vary systematically with position along the trailing pool boundary: R = v travel ⋅ cos θ R = v_{\text{travel}} \cdot \cos\theta R = v travel ⋅ cos θ
where θ \theta θ is the angle between the welding travel direction and the normal to the solidification front.
At the Fusion Boundary ( θ ≈ 90 ∘ \theta \approx 90^\circ θ ≈ 9 0 ∘ ): The growth rate R → 0 R \to 0 R → 0 , while the thermal gradient into the cold base metal ( G L G_L G L ) is at its absolute maximum. Therefore, G L / R → ∞ G_L / R \to \infty G L / R → ∞ . A thin layer of planar or fine cellular growth initiates epitaxially from the base-metal grains.
Between Fusion Boundary and Centerline: As the interface advances, θ \theta θ decreases toward 0 ∘ 0^\circ 0 ∘ . The growth velocity R R R accelerates toward v travel v_{\text{travel}} v travel , while the thermal gradient G L G_L G L flattens due to heat accumulation in the trailing liquid. G L / R G_L / R G L / R plunges by orders of magnitude, triggering rapid breakdown into columnar dendritic morphology.
At the Weld Centerline ( θ = 0 ∘ \theta = 0^\circ θ = 0 ∘ ): Growth rate reaches its maximum ( R = v travel R = v_{\text{travel}} R = v travel ) and G L G_L G L drops to its minimum. G L / R G_L / R G L / R reaches its lowest value across the weld. If constitutional supercooling is sufficiently intense and heterogeneous nucleants are present, equiaxed dendrites nucleate in the liquid ahead of the advancing columnar fronts, blocking competitive columnar impingement.
Microsegregation Dynamics & The Scheil Equation
Solidification in welds occurs too rapidly for solid-state diffusion to homogenize the growing crystals. Non-equilibrium solute redistribution is governed by the classical Scheil-Gulliver equation , derived under three fundamental metallurgical assumptions:
Negligible diffusion in the solid phase ( D S ≈ 0 D_S \approx 0 D S ≈ 0 ).
Complete, instantaneous diffusion and convective mixing in the liquid phase ( D L → ∞ D_L \to \infty D L → ∞ ).
Local thermodynamic equilibrium maintained at the solid-liquid interface ( C s ∗ = k ⋅ C L C_s^* = k \cdot C_L C s ∗ = k ⋅ C L ). SCHEIL SOLUTE REDISTRIBUTION
- Solute Concentration (C) ^
- | Terminal Eutectic
- | Liquid Film
- | |
- | v
- | |--|
- | C_L(f_s) | |
- | /-------+--|
- | / | |
- | C_s(f_s)/ | |
- C_0 +-----------------------------/----------+--|
- | ..---------' | |
- k*C_0 +----------------' | |
- +----------------------------------------+--+--->
- 0.0 Solid Fraction (f_s) 1.0
- The Mathematical Formulation
The solute concentration in the solid at solid fraction f s f_s f s ( 0 ≤ f s < 1 0 \le f_s < 1 0 ≤ f s < 1 ) is given by: C s = k C 0 ( 1 − f s ) k − 1 C_s = k C_0 (1 - f_s)^{k - 1} C s = k C 0 ( 1 − f s ) k − 1
The solute concentration in the remaining liquid pool is: C L = C 0 ( 1 − f s ) k − 1 C_L = C_0 (1 - f_s)^{k - 1} C L = C 0 ( 1 − f s ) k − 1
Segregation of Tramp Elements and Hot Cracking
For solutes with equilibrium partition coefficients far below unity ( k ≪ 1 k \ll 1 k ≪ 1 ), solute rejection is extreme:
Sulfur in Iron: k S ≈ 0.05 k_S \approx 0.05 k S ≈ 0.05 .
Phosphorus in Iron: k P ≈ 0.06 k_P \approx 0.06 k P ≈ 0.06 .
Carbon in Iron ( δ \delta δ -ferrite): k C ≈ 0.19 k_C \approx 0.19 k C ≈ 0.19 .
As solidification proceeds toward completion ( f s > 0.90 to 0.98 f_s > 0.90\text{ to }0.98 f s > 0.90 to 0.98 ), sulfur and phosphorus are rejected into the shrinking interdendritic liquid channels. When f s = 0.98 f_s = 0.98 f s = 0.98 , the concentration of sulfur in the remaining liquid spikes by a factor of: C L C 0 = ( 1 − 0.98 ) 0.05 − 1 = ( 0.02 ) − 0.95 ≈ 40.7 \frac{C_L}{C_0} = (1 - 0.98)^{0.05 - 1} = (0.02)^{-0.95} \approx 40.7 C 0 C L = ( 1 − 0.98 ) 0.05 − 1 = ( 0.02 ) − 0.95 ≈ 40.7
A bulk sulfur level of just 0.020 wt % 0.020\text{ wt}\% 0.020 wt % enriches to > 0.80 wt % >0.80\text{ wt}\% > 0.80 wt % in the final liquid! This concentrated liquid forms low-melting eutectic phases (iron-iron sulfide eutectic, Fe − FeS \text{Fe}-\text{FeS} Fe − FeS , freezing at 988 ∘ C 988^\circ\text{C} 98 8 ∘ C , or iron phosphide, Fe 3 P \text{Fe}_3\text{P} Fe 3 P , freezing at 1050 ∘ C 1050^\circ\text{C} 105 0 ∘ C ).
Because pure steel solidifies at ∼ 1500 ∘ C \sim 1500^\circ\text{C} ∼ 150 0 ∘ C , these low-melting liquid films wet the columnar grain boundaries over a 500 ∘ C 500^\circ\text{C} 50 0 ∘ C temperature span while the surrounding weld metal contracts thermally. When solidification shrinkage tensile strains pull across these wetted boundaries, the liquid tears apart, producing solidification hot cracks .
The Metallurgical Countermeasure: The Mn/S Ratio
To neutralize sulfur-induced hot cracking, manganese is added to structural steels. Manganese possesses a vastly higher thermodynamic affinity for sulfur than iron ( Δ G MnS ≪ Δ G FeS \Delta G_{\text{MnS}} \ll \Delta G_{\text{FeS}} Δ G MnS ≪ Δ G FeS ): FeS + Mn ⇌ MnS + Fe \text{FeS} + \text{Mn} \rightleftharpoons \text{MnS} + \text{Fe} FeS + Mn ⇌ MnS + Fe
Manganese sulfide (MnS) freezes as discrete, high-melting refractory globules ( T m ≈ 1610 ∘ C T_m \approx 1610^\circ\text{C} T m ≈ 161 0 ∘ C ) that precipitate within the liquid before terminal solidification, preventing continuous wetting of grain boundaries. AWS standards mandate a minimum Mn/S \text{Mn/S} Mn/S ratio ≥ 25 to 30 \ge 25\text{ to }30 ≥ 25 to 30 (and ideally > 40 >40 > 40 in high-restraint joints) to ensure freedom from solidification cracking.
Weld Pool Pulsation and the Origin of Weld Ripples
AWS B5.16 Clause 8.3.4 lists the origin of weld ripples as a distinct metallurgy sub-topic, and the reason is that ripples are a free, continuous record of how the weld pool actually solidified.
A weld bead does not solidify as a smoothly retreating front. The trailing edge of the pool advances in discrete pulses , and each pulse freezes a thin arc-shaped ridge on the bead surface. Three mechanisms drive the pulsation:
Periodic variation in arc force. Metal transfer is inherently periodic. Each droplet detachment, each short-circuit event and each current pulse in a synergic waveform momentarily depresses and then releases the pool surface.
Surface-tension oscillation of the pool. A molten pool behaves as a damped oscillator with a natural frequency set by its mass and surface tension, so it rings after every disturbance.
Latent heat release. Solidification is not continuous: the pool supercools slightly, then releases latent heat as a layer freezes, briefly halting the front before it advances again.
Ripple spacing therefore carries information: ripple spacing ≈ travel speed pulsation frequency \text{ripple spacing} \approx \frac{\text{travel speed}}{\text{pulsation frequency}} ripple spacing ≈ pulsation frequency travel speed
- Ripple appearance What it indicates
- Fine, uniform, evenly spaced Stable arc, steady travel speed, consistent transfer
- Coarse and widely spaced High travel speed relative to pulsation frequency, or low-frequency globular transfer
- Irregular and erratic Unstable arc, inconsistent travel, or intermittent shielding loss
Sharply pointed arcs trailing far behind Elongated teardrop pool — the classic centreline solidification cracking geometry
The last row is the reason this topic belongs in metallurgy rather than in cosmetic inspection. Ripples map the instantaneous pool boundary, so a bead whose ripples form long, sharply pointed chevrons is telling you the pool was teardrop-shaped, that solute segregated to the centreline, and that centreline cracking risk is elevated. A rounded elliptical ripple pattern indicates a pool shape in which grains meet the centreline at a shallow angle and cracking risk is far lower.
In pulsed GTAW and pulsed GMAW the relationship becomes exact: one ripple is deposited per current pulse, so counting ripples over a measured length directly verifies the pulse frequency and travel speed actually used in production against the values recorded in the procedure.