Study guide
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility
Key Takeaways Explain This Topic AI
The iron-carbon system presents two distinct equilibria: the metastable Fe-Fe3C system (governing conventional steel welding, heat treatment, and microstructure prediction) and the thermodynamically stable Fe-Graphite system (relevant to cast irons and prolonged graphitizing service).
Pure iron undergoes allotropic transformations between BCC alpha ferrite (stable up to 912°C, max carbon solubility 0.022 wt%), FCC gamma austenite (912–1394°C, max carbon solubility 2.14 wt%), and BCC delta ferrite (1394–1538°C, max carbon solubility 0.09 wt%), with interstitial carbon solubility governed by crystal lattice interstitial site geometry.
The three invariant equilibrium reactions—peritectic at 1495°C (0.17 wt% C), eutectic at 1148°C (4.30 wt% C), and eutectoid at 727°C (0.77 wt% C)—dictate primary solidification structures, hot cracking susceptibility, and subcritical lamellar pearlite formation.
Last updated: September 2026
10.1 Iron-Carbon Equilibrium Diagram & Equilibrium Phase Transformations
Quick Answer: The iron-carbon phase diagram forms the thermodynamic foundation of steel welding metallurgy. While the stable system represents iron and graphite, structural steels operate according to the metastable iron-cementite ( Fe − Fe 3 C \text{Fe}-\text{Fe}_3\text{C} Fe − Fe 3 C ) diagram. Pure iron exhibits three allotropes: Body-Centered Cubic (BCC) α \alpha α -ferrite, Face-Centered Cubic (FCC) γ \gamma γ -austenite, and BCC δ \delta δ -ferrite. Austenite dissolves up to 2.14 wt % 2.14\text{ wt}\% 2.14 wt % carbon at 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C due to its spacious octahedral interstitial sites, whereas ferrite dissolves a maximum of only 0.022 wt % 0.022\text{ wt}\% 0.022 wt % carbon at 727 ∘ C 727^\circ\text{C} 72 7 ∘ C . Three invariant reactions govern phase changes: peritectic ( 1495 ∘ C 1495^\circ\text{C} 149 5 ∘ C , 0.17 % C 0.17\%\text{ C} 0.17% C ), eutectic ( 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C , 4.30 % C 4.30\%\text{ C} 4.30% C ), and eutectoid ( 727 ∘ C 727^\circ\text{C} 72 7 ∘ C , 0.77 % C 0.77\%\text{ C} 0.77% C ). Alloying elements modify these boundaries: austenite stabilizers (Ni, Mn, C, N) expand the γ \gamma γ -phase field, whereas ferrite stabilizers (Cr, Mo, Si, V, Ti) contract it, closing the γ \gamma γ -loop above critical concentrations.
The Fe-Fe3C Metastable vs. Fe-C Stable System
In steel welding metallurgy, thermodynamic equilibrium phase relationships are described by the binary iron-carbon system. Two distinct phase diagrams exist:
The Stable Iron-Graphite System ( Fe − C \text{Fe}-\text{C} Fe − C ): In this system, elemental carbon precipitates as hexagonal graphite. Graphite represents the true thermodynamic minimum in Gibbs free energy ( Δ G < 0 \Delta G < 0 Δ G < 0 ). However, graphite nucleation kinetics in solid steel are exceedingly sluggish, requiring extremely slow cooling rates (on the order of degrees per hour) or prolonged isothermal holding at elevated temperatures ( > 650 ∘ C >650^\circ\text{C} > 65 0 ∘ C ) in the presence of strong graphitizing elements such as silicon (e.g., in grey cast irons).
The Metastable Iron-Iron Carbide System ( Fe − Fe 3 C \text{Fe}-\text{Fe}_3\text{C} Fe − Fe 3 C ): Under all practical arc welding, thermomechanical processing, and conventional heat-treating thermal cycles, carbon precipitates as the metastable intermetallic compound cementite ( Fe 3 C \text{Fe}_3\text{C} Fe 3 C , or iron carbide). Because the free energy difference between cementite and graphite is small (approximately 3 to 5 kJ/mol 3\text{ to }5\text{ kJ/mol} 3 to 5 kJ/mol ), and the kinetic barrier to nucleating cementite is vastly lower than that of graphite, the metastable Fe − Fe 3 C \text{Fe}-\text{Fe}_3\text{C} Fe − Fe 3 C system governs the microstructural evolution of carbon and low-alloy structural steels. TEMPERATURE vs. PHASE STABILITY
- Liquid (L)
- | [1538°C Melting Point]
- v
- Delta (δ) Ferrite (BCC, a = 0.293 nm) ----> Peritectic Reaction at 1495°C (0.17% C)
- | [1394°C A4 Transition]
- v
- Gamma (γ) Austenite (FCC, a = 0.358 nm) --> Eutectic Reaction at 1148°C (4.30% C)
- | [912°C A3 Transition]
- v
- Alpha (α) Ferrite (BCC, a = 0.286 nm) ----> Eutectoid Reaction at 727°C (0.77% C)
- | [770°C A2 Curie Temperature (Magnetic Transition, No Phase Change)]
- v
- Room Temperature Equilibrium Microstructure (α-Ferrite + Fe3C Cementite / Pearlite)
- Crystal Structure, Lattice Parameters, c/a Ratio & Interstitial Sites
AWS B5.16 Clause 8.3.4 opens the metallurgy body of knowledge with crystal structure of metals (FCC, BCC, HCP, unit cells, lattice parameter, c/a ratio, atom positions, interstitial positions) . Every solubility limit and transformation temperature discussed above ultimately traces back to these lattices.
The Three Engineering Lattices
Lattice Atoms per unit cell Coordination number Atomic packing factor Close-packed planes / directions Welding-relevant metals
- BCC 2 8 0.68 {110} / ⟨111⟩ alpha-Fe, delta-Fe, ferritic and martensitic stainless, Mo, W, beta-Ti
- FCC 4 12 0.74 {111} / ⟨110⟩ gamma-Fe, austenitic stainless, Al, Ni, Cu
- HCP 6 12 0.74 (0001) / ⟨11-20⟩ alpha-Ti, Zn, Mg, Co, Zr
Lattice parameter is the edge length of the unit cell. For iron, alpha-ferrite measures a ≈ 0.2866 nm a \approx 0.2866\text{ nm} a ≈ 0.2866 nm at room temperature while gamma-austenite measures a ≈ 0.3647 nm a \approx 0.3647\text{ nm} a ≈ 0.3647 nm near 912 ∘ C 912^\circ\text{C} 91 2 ∘ C . The austenite cell is larger overall, yet austenite is the denser structure because it holds four atoms instead of two — the reason the volume contracts about 1% on heating through the A 3 \text{A}_3 A 3 transformation and expands on the reverse transformation, and the reason martensite formation expands a weldment and generates compressive transformation strain.
Atom positions are expressed in fractional cell coordinates: BCC has atoms at ( 0 , 0 , 0 ) (0,0,0) ( 0 , 0 , 0 ) and the body centre ( 1 2 , 1 2 , 1 2 ) (\tfrac12,\tfrac12,\tfrac12) ( 2 1 , 2 1 , 2 1 ) ; FCC adds face centres at ( 1 2 , 1 2 , 0 ) (\tfrac12,\tfrac12,0) ( 2 1 , 2 1 , 0 ) and equivalents; HCP places the basal atoms at ( 0 , 0 , 0 ) (0,0,0) ( 0 , 0 , 0 ) with the interior atom at ( 1 3 , 2 3 , 1 2 ) (\tfrac13,\tfrac23,\tfrac12) ( 3 1 , 3 2 , 2 1 ) .
The c/a Ratio
HCP metals are described by two lattice parameters — the basal edge a a a and the prism height c c c . The c/a ratio for ideal hard-sphere stacking is ( c a ) ideal = 8 3 = 1.633 \left(\frac{c}{a}\right)_{\text{ideal}} = \sqrt{\frac{8}{3}} = 1.633 ( a c ) ideal = 3 8 = 1.633
Real metals deviate, and the deviation predicts deformation behaviour that matters directly to weld ductility:
- Metal c/a Deviation Consequence
- Zinc 1.856 above ideal Basal slip only; brittle, poor weldability, galvanize burn-off
- Cobalt 1.623 near ideal Basal slip dominant
- Magnesium 1.624 near ideal Limited slip systems; hot cracking and tearing risk
- Titanium (alpha) 1.587 below ideal Prismatic slip activates; alpha-Ti is genuinely ductile and weldable
That single number explains why alpha-titanium weldments tolerate strain while zinc-rich coatings simply crack or vaporize.
Interstitial Positions and Why Carbon Behaves as It Does
Carbon, nitrogen, hydrogen, boron and oxygen dissolve interstitially , occupying the voids between iron atoms. The two void types have fixed radius ratios:
Octahedral site: accommodates a sphere with r / R = 0.414 r/R = 0.414 r / R = 0.414 in an FCC lattice.
Tetrahedral site: accommodates r / R = 0.225 r/R = 0.225 r / R = 0.225 in FCC, 0.291 0.291 0.291 in BCC.
FCC austenite has larger, more symmetric octahedral holes and dissolves up to 2.11 wt% C at 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C . BCC ferrite, despite being the more open structure by packing factor, has small, distorted octahedral sites and dissolves only 0.022 wt% C at 727 ∘ C 727^\circ\text{C} 72 7 ∘ C — a factor of roughly 100 lower. This single ratio drives the entire discipline: it is why rapid cooling traps carbon in a supersaturated body-centred-tetragonal martensite, why the tetragonality c / a c/a c / a of martensite rises with carbon content, and why hydrogen — small enough to hop between tetrahedral sites — diffuses orders of magnitude faster in ferrite than in austenite, which is the metallurgical basis of austenitic buttering layers for hydrogen control.
The Monotectic Reaction
Clause 8.3.4 lists four invariant reactions; the three iron-carbon reactions were covered above, and the fourth is the monotectic : L 1 → cooling S + L 2 L_1 \xrightarrow{\text{cooling}} S + L_2 L 1 cooling S + L 2
A single liquid decomposes into a solid plus a second, immiscible liquid of different composition. The classic system is copper-lead , which has a monotectic near 955 ∘ C 955^\circ\text{C} 95 5 ∘ C where a copper-rich liquid decomposes into FCC copper plus a lead-rich liquid; the liquid-lead phase persists to low temperature and is the basis of leaded bearing bronzes.
Monotectics matter to a welding engineer because the residual low-melting liquid is precisely what causes liquid metal embrittlement and hot shortness . Leaded free-machining steels, leaded brasses and leaded bronzes all retain a discrete lead-rich liquid phase far below the solidus of the matrix; welding them wets the grain boundaries ahead of the arc and produces intergranular cracking that no preheat or filler-metal change will fix. The correct engineering answer is a substitution — specify a bismuth-free, lead-free free-machining grade, or join by a solid-state or brazing process that never melts the matrix.
Exam Trap: Confusing monotectic with eutectic. Both start from a single liquid. A eutectic produces two solids ( L → S 1 + S 2 L \rightarrow S_1 + S_2 L → S 1 + S 2 ). A monotectic produces one solid and one liquid ( L 1 → S + L 2 L_1 \rightarrow S + L_2 L 1 → S + L 2 ). Any answer that describes a monotectic as yielding two solid phases is wrong.
Crystallographic Allotropes of Iron & Interstitial Solubility
Pure iron displays allotropy, transitioning between distinct crystallographic space groups as a function of temperature under atmospheric pressure:
1. Alpha Ferrite ( α \alpha α )
Crystal Structure: Body-Centered Cubic (BCC), space group I m 3 ˉ m Im\bar{3}m I m 3 ˉ m .
Stability Range: Ambient temperature up to 912 ∘ C 912^\circ\text{C} 91 2 ∘ C ( 1185 K 1185\text{ K} 1185 K ).
Lattice Parameter: a ≈ 0.2866 nm a \approx 0.2866\text{ nm} a ≈ 0.2866 nm ( 2.866 A ˚ 2.866\text{ \AA} 2.866 A ˚ ) at 20 ∘ C 20^\circ\text{C} 2 0 ∘ C .
Interstitial Carbon Solubility: Maximum of 0.022 wt % 0.022\text{ wt}\% 0.022 wt % ( 0.10 at % 0.10\text{ at}\% 0.10 at % ) at 727 ∘ C 727^\circ\text{C} 72 7 ∘ C , dropping to less than 0.008 wt % 0.008\text{ wt}\% 0.008 wt % at room temperature.
Lattice Geometry Rationale: In the BCC unit cell, the octahedral interstitial sites (located at unit cell face centers [ 1 2 , 1 2 , 0 ] [\frac{1}{2}, \frac{1}{2}, 0] [ 2 1 , 2 1 , 0 ] and edge centers [ 0 , 0 , 1 2 ] [0, 0, \frac{1}{2}] [ 0 , 0 , 2 1 ] ) are non-spherical and highly constrained. The radius of the largest sphere that fits into an octahedral site without lattice distortion is r o = 0.155 R Fe ≈ 0.019 nm r_o = 0.155 R_{\text{Fe}} \approx 0.019\text{ nm} r o = 0.155 R Fe ≈ 0.019 nm . The tetrahedral site radius is r t = 0.291 R Fe ≈ 0.036 nm r_t = 0.291 R_{\text{Fe}} \approx 0.036\text{ nm} r t = 0.291 R Fe ≈ 0.036 nm . Although the tetrahedral site is geometrically larger, carbon atoms ( r C ≈ 0.077 nm r_{\text{C}} \approx 0.077\text{ nm} r C ≈ 0.077 nm ) preferentially occupy the octahedral sites because displacement of only two nearest-neighbor iron atoms along the ⟨ 100 ⟩ \langle 100 \rangle ⟨ 100 ⟩ direction accommodates the carbon atom, producing severe tetragonal strain. This pronounced elastic strain field severely restricts carbon solid solubility in α \alpha α -ferrite.
2. Gamma Austenite ( γ \gamma γ )
Crystal Structure: Face-Centered Cubic (FCC), space group F m 3 ˉ m Fm\bar{3}m F m 3 ˉ m .
Stability Range: 912 ∘ C 912^\circ\text{C} 91 2 ∘ C to 1394 ∘ C 1394^\circ\text{C} 139 4 ∘ C ( 1185 to 1667 K 1185\text{ to }1667\text{ K} 1185 to 1667 K ).
Lattice Parameter: a ≈ 0.3585 nm a \approx 0.3585\text{ nm} a ≈ 0.3585 nm ( 3.585 A ˚ 3.585\text{ \AA} 3.585 A ˚ ) at 912 ∘ C 912^\circ\text{C} 91 2 ∘ C .
Interstitial Carbon Solubility: Maximum of 2.14 wt % 2.14\text{ wt}\% 2.14 wt % ( 9.2 at % 9.2\text{ at}\% 9.2 at % ) at 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C , decreasing to 0.77 wt % 0.77\text{ wt}\% 0.77 wt % at the eutectoid temperature ( 727 ∘ C 727^\circ\text{C} 72 7 ∘ C ).
Lattice Geometry Rationale: The FCC lattice possesses symmetric, spherical octahedral interstitial sites located at the center of the unit cell [ 1 2 , 1 2 , 1 2 ] [\frac{1}{2}, \frac{1}{2}, \frac{1}{2}] [ 2 1 , 2 1 , 2 1 ] and at the midpoints of all 12 cube edges. The octahedral radius is r o = 0.414 R Fe ≈ 0.053 nm r_o = 0.414 R_{\text{Fe}} \approx 0.053\text{ nm} r o = 0.414 R Fe ≈ 0.053 nm , surrounded by six equidistant iron atoms. Accommodating a carbon atom ( 0.077 nm 0.077\text{ nm} 0.077 nm ) requires modest isotropic lattice expansion, allowing austenite to dissolve nearly 100 × 100\times 100 × more carbon than ferrite.
3. Delta Ferrite ( δ \delta δ )
Crystal Structure: Body-Centered Cubic (BCC), identical crystallographic symmetry to α \alpha α -ferrite.
Stability Range: 1394 ∘ C 1394^\circ\text{C} 139 4 ∘ C up to the congruent melting point of pure iron at 1538 ∘ C 1538^\circ\text{C} 153 8 ∘ C ( 1667 to 1811 K 1667\text{ to }1811\text{ K} 1667 to 1811 K ).
Lattice Parameter: a ≈ 0.293 nm a \approx 0.293\text{ nm} a ≈ 0.293 nm at 1400 ∘ C 1400^\circ\text{C} 140 0 ∘ C due to thermal lattice expansion.
Interstitial Carbon Solubility: Maximum of 0.09 wt % 0.09\text{ wt}\% 0.09 wt % at 1495 ∘ C 1495^\circ\text{C} 149 5 ∘ C . The expanded lattice enables higher interstitial solubility than α \alpha α -ferrite, but it remains far lower than that of γ \gamma γ -austenite.
4. Cementite ( Fe 3 C \text{Fe}_3\text{C} Fe 3 C )
Crystal Structure: Complex Orthorhombic, space group P n m a Pnma P nma , containing 12 iron atoms and 4 carbon atoms per unit cell ( a = 0.509 nm a = 0.509\text{ nm} a = 0.509 nm , b = 0.674 nm b = 0.674\text{ nm} b = 0.674 nm , c = 0.452 nm c = 0.452\text{ nm} c = 0.452 nm ).
Stoichiometry: Fixed carbon concentration of 6.70 wt % 6.70\text{ wt}\% 6.70 wt % ( 25.0 at % 25.0\text{ at}\% 25.0 at % ).
Mechanical Characteristics: Extremely hard ( > 800 to 1000 HV >800\text{ to }1000\text{ HV} > 800 to 1000 HV ) and brittle, with negligible room-temperature tensile ductility. Acts as the primary strengthening constituent in pearlitic and bainitic microstructures.
Phase / Constituent Crystal System Space Group Max Carbon Solubility (wt%) Temperature of Max Solubility Density (g/cm³)
α \alpha α -Ferrite BCC I m 3 ˉ m Im\bar{3}m I m 3 ˉ m 0.022 % 0.022\% 0.022% 727 ∘ C 727^\circ\text{C} 72 7 ∘ C 7.87 7.87 7.87
γ \gamma γ -Austenite FCC F m 3 ˉ m Fm\bar{3}m F m 3 ˉ m 2.14 % 2.14\% 2.14% 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C 8.05 8.05 8.05
δ \delta δ -Ferrite BCC I m 3 ˉ m Im\bar{3}m I m 3 ˉ m 0.09 % 0.09\% 0.09% 1495 ∘ C 1495^\circ\text{C} 149 5 ∘ C 7.35 7.35 7.35
Cementite ( Fe 3 C \text{Fe}_3\text{C} Fe 3 C ) Orthorhombic P n m a Pnma P nma 6.70 % 6.70\% 6.70% (Fixed) Up to 1227 ∘ C 1227^\circ\text{C} 122 7 ∘ C (decomp.) 7.67 7.67 7.67
Pearlite Lamellar α + Fe 3 C \alpha + \text{Fe}_3\text{C} α + Fe 3 C Aggregate 0.77 % 0.77\% 0.77% (Eutectoid) Formed at 727 ∘ C 727^\circ\text{C} 72 7 ∘ C 7.85 7.85 7.85