Study guide

11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing

AWS CWEng Certified Welding Engineer Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction & CWEng Exam Overview

About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set

2 Chapter 1: Mathematics & Statistics for Welding Engineers

1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers

3 Chapter 2: Physics Fundamentals & Mechanics

2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity

4 Chapter 3: General & Physical Chemistry for Welding

3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection

5 Chapter 4: Strength of Materials & Mechanics of Materials

4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment

6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding

5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments

7 Chapter 6: Electrical Engineering Principles for Welding Systems

6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow

8 Chapter 7: Welding Heat Sources & Arc Physics

7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design

9 Chapter 8: Arc Welding Processes & Parameter Controls

8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems

10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes

9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray

11 Chapter 10: Physical & Transformation Metallurgy of Steels

10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control

12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy

11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences

13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics

12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control

14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis

13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction

15 Chapter 14: Brazing, Soldering & Industrial Welding Safety

14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation

16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation

15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice

17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1

16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation

18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control

17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing

19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics

18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison

11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing

Key Takeaways Explain This Topic AI

Solidification cracking occurs at terminal dendritic solidification within the Brittle Temperature Range (BTR) due to low-melting liquid films (Fe-FeS and Fe-Fe3P eutectics) that cannot accommodate transverse thermal contraction strains.

A weld bead depth-to-width (D/W) ratio greater than 1.0 creates a severe centerline plane of weakness where advancing columnar dendrites meet at sharp angles, trapping segregated liquid films and causing centerline hot cracks.

Liquation cracking occurs in the subsolidus Heat-Affected Zone (partially melted zone) due to constitutional liquation of grain boundary sulfides, phosphides, or carbides under thermal contraction stresses.

Last updated: September 2026

11.2 Hot Cracking (Solidification/Liquation) & Lamellar Tearing Mechanisms

Quick Answer: Hot cracking encompasses high-temperature fractures occurring during the solidification of weld metal or localized melting within the subsolidus Heat-Affected Zone (HAZ). Solidification cracking occurs along the fusion zone centerline within the Brittle Temperature Range (BTR) when low-melting liquid eutectic films (primarily iron sulfides Fe-FeS and phosphides Fe-Fe3P) are pulled apart by transverse thermal contraction strains; it is suppressed by enforcing an Mn/S ratio > 25 to 30, limiting P + S <= 0.015%, and maintaining a depth-to-width (D/W) ratio < 0.8. Liquation cracking occurs in the partially melted zone (PMZ) via constitutional liquation of boundary precipitates. In contrast, lamellar tearing is a mechanical, through-thickness step-like fracture in heavy rolled plates (thickness > 25 mm) driven by high Z-direction shrinkage stresses acting across rolled-out, planar Type II MnS inclusion stringers, requiring "Z-grade" steels (ASTM A770), buffer layers, or joint redesign.

Solidification Cracking: Thermodynamics & Metallurgy

Solidification cracking (also termed hot tearing or centerline cracking) occurs in the weld metal fusion zone during the terminal stages of dendritic crystallization, specifically within the Brittle Temperature Range (BTR) : BTR = T_liquidus - T_coherence/solidus

where T_coherence is the coherence temperature at which growing solid dendrites touch and interlock (fraction solid f_s approx 0.70 to 0.90), preventing free liquid feeding to relieve thermal contraction. DENDRITIC SOLIDIFICATION & LIQUID FILMS

  • Advancing Solid Dendrites Interdendritic Liquid Films
  • +-----------------------+ (Segregated FeS, Fe3P, BTR)
  • | Solid Martensite / | |
  • | Ferrite Dendrites | v
  • | \\\\\\\\\\\\\ | |~~~~~~~~~~~~|
  • +-----------------------+ | Liquid | <-- Contraction
  • -> <-- | Interlayer | Strain (epsilon)
  • Thermal Contraction |~~~~~~~~~~~~| Pulls Film

Tensile Stresses +------------+ Apart!

  • +-----------------------+ |
  • | Solid Martensite / | v
  • | Ferrite Dendrites | CENTERLINE HOT CRACK

| ///////////// | FORMS AT SOLIDUS!

  • +-----------------------+
  • Solute Redistribution & Equilibrium Partition Coefficient

As solid grains solidify, solute elements are rejected from the advancing solid front into the remaining interstitial liquid in accordance with the equilibrium partition coefficient (k_0): k_0 = C_s / C_L

where C_s and C_L are the solute concentrations in the solid and liquid phases at equilibrium. Elements with extremely low partition coefficients (k_0 << 1.0) segregate heavily into the last remaining liquid at dendrite boundaries and along the weld centerline:

Sulfur (k_0 approx 0.05 in austenite): Forms an iron-iron sulfide eutectic (Fe-FeS) that solidifies at a remarkably low temperature of 988°C (1810°F) —more than 500°C below the solidus of unalloyed steel (1538°C).

Phosphorus (k_0 approx 0.06 in austenite): Forms an iron-iron phosphide eutectic (Fe-Fe3P) melting at 1050°C (1922°F) .

Carbon, Boron, and Niobium: Further widen the BTR and depress terminal liquid freezing points.

Because these thin liquid interlayers wet the solid dendritic boundaries over a broad temperature range, the cohesive strength of the mushy zone is practically zero. When transverse thermal contraction strains exceed the critical fracture strain of the mushy boundary (epsilon_thermal > epsilon_fracture), the liquid film tears open, creating an intergranular/interdendritic solidification crack.

The Critical Role of the Manganese-to-Sulfur Ratio (Mn/S)

To suppress the low-melting Fe-FeS eutectic, sufficient manganese must be present in the weld deposit to drive the high-temperature chemical reaction: FeS + Mn -> MnS + Fe

Manganese sulfide (MnS) possesses a high melting point of 1610°C (2930°F) , well above the liquidus of structural steel. Consequently, MnS precipitates early during solidification as discrete, harmless, spherical/globular inclusions floating within dendrite cores, consuming sulfur before low-melting boundary films can form.

Engineering Rule: To guarantee complete suppression of FeS wetting films, the manganese-to-sulfur ratio must satisfy: Mn / S >= 25 to 30

For high-restraint joints, carbon-manganese steel weld metals should maintain Mn/S > 35 with total phosphorus and sulfur constrained to [P] + [S] <= 0.015% to 0.020%.

Bead Geometry & Weld Pool Aspect Ratio

Solidification cracking is intimately coupled with the macroscopic shape of the weld pool and the resulting bead geometry. BEAD ASPECT RATIO & GRAIN IMPINGEMENT

  • DEEP / NARROW (D/W > 1.0) WIDE / CONVEX (D/W < 0.8)
  • [ High Hot Crack Risk ] [ Crack-Resistant ]
  • Bead Width (W) Bead Width (W)
  • |<--------------->| |<------------------->|
  • + + + +
  • | \ / | \ /
  • | \ | / | \ /
  • | \ | / | \ ^ /
  • Depth | \ v / | Depth \ / \ /
  • (D) | \ | / | (D) \ / \ /
  • | \ | / | +---+---+---+
  • +-------v-+-------+ v
  • Centerline Crack Curved, interlocking
  • traps low-melting dendrites bridge pool

liquid eutectics! without planar seam!

Depth-to-Width Ratio (D/W)

Deep, Narrow Beads (D/W > 1.0): Typical of high-current Submerged Arc Welding (SAW), keyhole plasma/laser welding, or narrow-gap root passes. The thermal gradient drives columnar dendrites to grow perpendicular to the retreating pool boundaries. In deep, narrow grooves, opposing dendrites from opposite sidewalls meet abruptly along a single, planar vertical line at the joint center. All rejected low-melting solutes (S, P) are swept into this centerline plane of impingement, producing severe centerline solidification cracks.

Wide, Convex Beads (D/W = 0.5 to 0.8, or W/D >= 1.25): Columnar dendrites grow upward and inward with curved trajectories, creating an interlocking, staggered cellular pattern that allows continuous liquid feeding to backfill shrinkage voids without forming a continuous planar weak seam.

Bead Surface Contour (Convex vs. Concave)

Concave Bead Caps: Thermal shrinkage places the outer surface of a concave fillet or groove weld under extreme transverse tension during terminal solidification, pulling surface liquid films apart.

Convex Bead Caps: Thermal shrinkage exerts internal compressive forces across the cap center, suppressing hot crack opening.

Travel Speed & Pool Geometry (Elliptical vs. Tear-Drop)

High Travel Speed: Stretches the molten pool into an elongated tear-drop shape with a sharp, pointed trailing boundary. Dendrites grow perpendicular to the pool boundary and meet at a sharp 90° impingement angle along the centerline, promoting cracking.

Moderate Travel Speed: Maintains an elliptical pool contour where dendrites curve gradually toward the welding axis, interlocking smoothly along the weld axis.

Liquation Cracking in the Heat-Affected Zone (HAZ)

Liquation cracking (also termed hot micro-fissuring) occurs in the solid Heat-Affected Zone immediately adjacent to the fusion boundary—a microstructural subzone known as the Partially Melted Zone (PMZ) . Unlike solidification cracking, which occurs in the molten pool, liquation cracking occurs in the base metal matrix that remained solid during the welding cycle. CONSTITUTIONAL LIQUATION IN HAZ (PMZ)

  • Molten Pool | Fusion Boundary | Partially Melted Zone (PMZ)
  • | |
  • Liquid | Solid Coarse | Secondary Phase Precipitate (e.g., FeS, NbC)

Weld Metal | Austenite | reacts with surrounding matrix at T_eutectic < T_solidus!

  • | Grains |
  • | | [ Solid Matrix ]
  • | | / \
  • | | ( Liquated Film )
  • | | \ along Grain /
  • | | [ Boundary ]
  • | | |
  • | | v
  • | | PULLS APART UNDER

| | CONTRACTION STRESS!

Mechanism of Constitutional Liquation

Constitutional liquation occurs when secondary-phase precipitate particles (e.g., niobium carbides NbC, titanium carbonitrides Ti(C,N), iron sulfides FeS, or chromium borides) react eutectically with the surrounding solid iron or nickel matrix during rapid heating:

During rapid welding thermal cycles, solid-state dissolution of precipitates cannot proceed to completion before reaching the eutectic temperature T_eutectic.

At T_peak >= T_eutectic (which is lower than the equilibrium solidus of the alloy), a localized liquid film forms at the precipitate-matrix interface.

This liquid film rapidly wets along prior-austenite grain boundaries via capillary action, forming continuous grain boundary liquid films.

As the adjacent weld metal solidifies and contracts, transverse tensile stresses pull these liquated grain boundaries apart, generating microscopic intergranular fissures (0.1 to 1.0 mm long).

Liquation cracking is especially prevalent in precipitation-strengthened nickel superalloys (Inconel 718, Waspaloy), fully austenitic stainless steels, and high-strength microalloyed steels with high niobium ([Nb] > 0.04%) or boron contents.

Lamellar Tearing: Mechanics, Inclusions & Joint Restraint

Lamellar tearing is a catastrophic, step-like subsurface cracking phenomenon occurring parallel to the rolling plane of heavy structural rolled steel plates (typically thicknesses t >= 25 to 50 mm). It occurs primarily beneath welded T-joints, corner joints, and cruciform connections where full-penetration groove welds impose high through-thickness (Z-direction / short-transverse) tensile contraction stresses . LAMELLAR TEARING MORPHOLOGY

  • Attached Flange / Stiffener
  • | |
  • | |
  • | |
  • +----+---+----+
  • | | | |
  • Weld | / \ | Weld
  • Metal | / \ | Metal
  • +-+---------+-+
  • ==================+=========+================== Main Plate Surface
  • ----------------------------------------------
  • -- [Planar Decollimations along MnS Stringers] (Terraces)
  • | |
  • v (Vertical Shear Tears) v
  • ----------------------------------------------
  • =============================================== Plate Bottom Surface
  • The Three Necessary Conditions for Lamellar Tearing

Susceptible Plate Material: Rolled plate containing high volume fractions of non-metallic, planar inclusions oriented parallel to the rolling surface.

High Through-Thickness Tensile Stress: Weld design and joint restraint that orient weld shrinkage vectors perpendicular to the rolling plane (the Z-axis / short-transverse direction).

Unfavorable Joint Configuration: Rigid connections (e.g., thick diaphragm-to-box columns, heavy nozzle necks) that concentrate shrinkage strains within a narrow through-thickness band.

Role of Non-Metallic Inclusions

During ingoting and continuous casting, non-metallic inclusions solidify. Subsequent heavy hot-rolling flattens these inclusions into broad, planar platelets or "stringers":

Type II Manganese Sulfides (MnS): Highly plastic at hot-rolling temperatures (1000°C to 1200°C); roll into elongated, paper-thin ribbons or flattened sheets.

Silicates (SiO2 complexes): Deform into thin, brittle planar disks.

Alumina Clusters (Al2O3): Line up in stringers along rolling flow lines.

Under through-thickness tensile stress, decohesion occurs along the weak inclusion-matrix interfaces, generating horizontal planar microcracks ("terraces"). As strain accumulates, the intervening vertical ligaments between adjoining terraces fail by shear ductile overload, linking the terraces into a macroscopic, step-like "terrace-and-wall" fracture.