11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control

AWS CWEng Certified Welding Engineer Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction & CWEng Exam Overview

About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set

2 Chapter 1: Mathematics & Statistics for Welding Engineers

1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers

3 Chapter 2: Physics Fundamentals & Mechanics

2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity

4 Chapter 3: General & Physical Chemistry for Welding

3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection

5 Chapter 4: Strength of Materials & Mechanics of Materials

4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment

6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding

5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments

7 Chapter 6: Electrical Engineering Principles for Welding Systems

6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow

8 Chapter 7: Welding Heat Sources & Arc Physics

7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design

9 Chapter 8: Arc Welding Processes & Parameter Controls

8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems

10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes

9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray

11 Chapter 10: Physical & Transformation Metallurgy of Steels

10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control

12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy

11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences

13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics

12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control

14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis

13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction

15 Chapter 14: Brazing, Soldering & Industrial Welding Safety

14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation

16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation

15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice

17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1

16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation

18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control

17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing

19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics

18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison

11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control

Key Takeaways Explain This Topic AI

Hydrogen-Induced Cold Cracking (HICC) requires the simultaneous presence of four necessary and sufficient conditions: a susceptible high-hardness microstructure (>350 HV), critical diffusible hydrogen (>5-15 mL/100g), tensile residual stress near yield magnitude, and an active temperature window between -100°C and +200°C.

The IIW Carbon Equivalent (CE_IIW) formula governs medium-to-high carbon steels (C >= 0.18%), whereas the Ito-Bessyo parameter (Pcm) is strictly required for modern low-carbon microalloyed and TMCP pipeline steels (C < 0.18%).

Diffusible hydrogen classifications follow AWS A4.3 and ISO 3690, spanning H16 (<=16 mL/100g), H8 (<=8 mL/100g), H4 (<=4 mL/100g), and ultra-clean H2 levels, measured primarily via gas chromatography or mercury displacement.

Last updated: September 2026

11.1 Carbon Equivalency (CE), Hydrogen-Induced Cold Cracking & Diffusible H2

Quick Answer: Hydrogen-Induced Cold Cracking (HICC)—variously designated as cold cracking, delayed cracking, or underbead cracking—is a catastrophic failure mechanism in ferritic and martensitic steels. It occurs only when four conditions exist concurrently : a susceptible microstructure (coarse-grained HAZ martensite or bainite with hardness > 350 HV), critical concentrations of diffusible hydrogen (H_diff > 5 to 15 mL/100g), tensile residual stress fields approaching yield magnitude, and an active embrittlement temperature between -100°C and +200°C (peaking near ambient). Eliminating any single factor prevents cracking, which is achieved industrially through carbon equivalent evaluation (CE_IIW vs. Pcm), low-hydrogen consumable management (H4/H8 ratings), calibrated preheat, and post-weld dehydrogenation heat treatment (DHT).

Phenomenological Mechanics: The Four Necessary and Sufficient Conditions

HICC is a delayed failure mechanism . Unlike solidification or hot cracking, which initiates during terminal liquid-phase crystallization, cold cracks initiate hours or days after the joint has reached ambient temperature—often during non-destructive examination (NDE) or hydrotesting. For high-strength quenched and tempered (Q&T) steels such as ASTM A514/A517, structural welding codes (e.g., AWS D1.1 Clause 8) mandate a minimum 48-hour inspection delay post-weld to allow delayed microcracks to propagate to detectable dimensions. THE FOUR TRIADS OF HYDROGEN CRACKING

  • [ Susceptible Microstructure ]
  • (Hardness > 350-380 HV,
  • Untempered Martensite)
  • / \
  • / \
  • / \
  • / HIC \
  • / REGION \
  • / \
  • [ Diffusible Hydrogen ] ---+-------------+--- [ Tensile Residual Stress ]
  • (> 5 to 15 mL/100g, (Yield Magnitude Stress,
  • Electrode moisture, Triaxial Notches at Root/Toe)
  • Grease, Primer)
  • |
  • v
  • [ Temperature Regime ]
  • (-100°C < T < +200°C;
  • Peak at -50°C to +50°C)
  • 1. Susceptible Microstructure

The transformation product most vulnerable to hydrogen embrittlement is untempered, high-carbon twinned martensite , followed in descending order of susceptibility by low-carbon lath martensite, lower bainite, upper bainite, and ferrite-pearlite. Coarse-grained heat-affected zones (CGHAZ, adjacent to the fusion boundary where peak temperatures exceed 1100°C to 1300°C) experience substantial austenite grain coarsening (ASTM grain size <= 3), which retards ferrite nucleation kinetics and enhances hardenability upon cooling.

Hardness Criteria: General engineering practice identifies a peak HAZ hardness threshold of 350 HV (Vickers 10-kg load) or approximately 35 HRC as the boundary above which cold cracking risk surges.

Sour Service Limits: Under NACE MR0175 / ISO 15156 environments containing wet H2S, environmental hydrogen uptake is severe; peak hardness in weld and HAZ is restricted to <= 250 HV (22 HRC) to prevent Sulfide Stress Cracking (SSC).

2. Diffusible Hydrogen Concentration (H_diff)

Hydrogen exists in weld deposits in two distinct thermodynamic states:

Diffusible Hydrogen (H_diff): Interstitial hydrogen ions (protons, H+) that diffuse freely through the interstitial octahedral and tetrahedral lattice sites of the BCC/BCT iron lattice at room temperature (diffusion coefficient D_H approx 10^-6 to 10^-7 cm^2/s). Driven by chemical potential gradients, diffusible hydrogen migrates toward regions of maximum hydrostatic tensile stress (triaxial stress fields ahead of crack tips, root notches, and inclusions).

Trapped Hydrogen (H_trap): Hydrogen captured in physical and metallurgical traps:

Reversible Traps: Low binding energy (E_b < 30 kJ/mol), such as dislocations, low-angle grain boundaries, and coherent precipitates. Hydrogen can desorb back into the matrix as temperature rises.

Irreversible Traps: High binding energy (E_b > 60 kJ/mol), such as incoherent interfaces of titanium carbonitrides Ti(C,N), manganese sulfides (MnS), complex oxide inclusions, and void cavities.

3. Tensile Residual Stress Fields

Welding generates localized, unyielding thermal contraction strains. In rigid, highly restrained structures (e.g., thick butt welds, cruciform joints, nozzle-to-shell connections), transverse tensile residual stresses invariably equal or exceed the room-temperature yield strength (sigma_residual approx R_p0.2) of the base or weld metal. Triaxial stress states at geometric discontinuities (weld toe re-entrant angles, root concavity, incomplete penetration) amplify local stresses by stress concentration factors (K_t = 2.0 to > 5.0), driving localized plastic dilation and dilation-induced hydrogen accumulation.

4. Active Temperature Window

Hydrogen embrittlement operates within a bounded temperature window: -100°C <= T <= +200°C , exhibiting a pronounced maximum susceptibility near room temperature (-50°C to +50°C):

Above +200°C: The kinetic mobility of hydrogen is extremely high (D_H > 10^-4 cm^2/s), preventing critical accumulation at localized stress concentrations. Dislocation slip occurs freely without dislocation-pinning embrittlement.

Below -100°C: Diffusion kinetics are frozen; hydrogen cannot migrate through the lattice toward crack-tip process zones during normal loading timeframes.

Carbon Equivalent Formulations & Metallurgy

Carbon equivalency formulas synthesize complex alloy chemistries into a single numerical index reflecting the hardenability and cracking susceptibility of the steel relative to unalloyed carbon steel.

Formula Designation Mathematical Expression Applicable Carbon Range Primary Industrial Application

IIW Carbon Equivalent (International Institute of Welding) CE_IIW = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15 C >= 0.18 wt% Structural C-Mn steels, heavy forgings, ASTM A36, A516, A572 (traditional)

Ito-Bessyo Cracking Parameter (Pcm) Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5*B C < 0.18 wt% Modern low-carbon microalloyed, TMCP, API 5L line pipe (X65 to X100)

Yurioka CEN Formula (Universal Parameter) CEN = C + A(C) * [Si/24 + Mn/6 + Cu/15 + Ni/20 + (Cr + Mo + Nb + V)/5 + 5*B] Universal (0.05% <= C <= 0.40%) Bridges low-carbon and high-carbon behaviors seamlessly

In Yurioka's equation, the accommodation function A(C) transitions smoothly between low- and high-carbon regimes: A(C) = 0.75 + 0.25 * tanh[20 * (C - 0.12)]

When C <= 0.08%, A(C) approaches 0.50, heavily discounting the hardenability potency of substitutional elements (matching Pcm weighting).

When C >= 0.18%, A(C) approaches 1.00, reproducing the full alloying coefficients of CE_IIW.

Hardenability Assessment Rules of Thumb (IIW Formula)

CE_IIW < 0.35% : Excellent weldability; preheat is generally unnecessary except for thick, highly restrained joints.

0.35% <= CE_IIW <= 0.45% : Moderate hardenability; preheat (50°C to 150°C) and low-hydrogen consumables (H8 or lower) are standard requirements.

CE_IIW > 0.45% : High hardenability; significant risk of martensite formation in the HAZ. Mandatory preheat (150°C to 250°C), strict interpass controls, H4 consumables, and post-weld dehydrogenation or stress relief are required. IIW CE vs. Pcm SELECTION CRITERIA FLOWCHART

  • [ Base Metal Chemistry ]
  • |

Is Carbon >= 0.18 wt% ?

  • / \
  • YES / \ NO
  • / \
  • v v
  • [ Use CE_IIW ] [ Use Pcm ]
  • C-Mn Steels TMCP / Microalloyed
  • ASTM A36, A516 API 5L X70/X80
  • Diffusible Hydrogen Measurement & Consumable Control
  • Diffusible Hydrogen Classification Scale

AWS filler metal specifications (e.g., AWS A5.1, A5.5, A5.18, A5.20) and ISO 14341 classify consumables with optional supplemental designators denoting the maximum diffusible hydrogen content per 100 grams of deposited weld metal:

H16 (Standard Low Hydrogen): <= 16.0 mL / 100g deposited metal. Basic electrodes (E7018) exposed to normal ambient humidity.

H8 (Controlled Low Hydrogen): <= 8.0 mL / 100g deposited metal. Standard requirement for high-restraint structural steel.

H4 (Ultra-Low Hydrogen): <= 4.0 mL / 100g deposited metal. Mandatory for high-strength quenched and tempered steels (e.g., ASTM A514, HY-80, S690QL).

H2 (Military / Submarine Grade): <= 2.0 mL / 100g deposited metal. Advanced aerospace and naval systems (HY-100, HSLA-100) under NAVSEA TechPub 248.

Standard Measurement Procedures (AWS A4.3 & ISO 3690) MERCURY DISPLACEMENT APPARATUS

  • [ Inverted Burette ]
  • | (Graduated)
  • | [ H2 Gas Cap ]
  • | |
  • || | || v
  • || v || Meniscus reading
  • || ||
  • ======++---++======
  • | Liquid Mercury |
  • | (Hg) |
  • | |
  • | [Weld Sample] | (Sample quenched,
  • | in bath base | cleaned, and held
  • +-----------------+ at 20-25°C for 72 hr)

Mercury Displacement Method (ISO 3690 Primary Reference): A welded test coupon (15 mm x 30 mm x 10 mm) is rapidly ice-water quenched, liquid-nitrogen cleaned, and placed beneath an inverted, mercury-filled graduated glass capillary burette. The assembly is held at 20°C to 25°C for 72 hours. Diffusing hydrogen effuses from the sample, rises through the dense liquid mercury, and collects in the closed upper capillary, displacing mercury to provide a volumetric reading. While historically considered the absolute analytical benchmark, mercury vapor toxicity has led to its restriction or prohibition in many commercial laboratories.

Gas Chromatography (GC) Method (AWS A4.3 / ISO 3690): The welded test coupon is sealed in an inert diffusion cell purged with high-purity argon or nitrogen carrier gas. The cell is heated to 150°C (for 6 hours) or up to 400°C to drive off diffusible hydrogen without desorbing deep, irreversibly trapped hydrogen. Effusing gas is swept through a molecular sieve column into a Thermal Conductivity Detector (TCD). The GC method is rapid, highly reproducible, environmentally safe, and measures hydrogen concentrations down to < 0.5 mL/100g.

Glycerin Displacement Method (Prohibited): The historical practice of collecting hydrogen over warm glycerin (45°C) is strictly prohibited by modern welding standards (AWS, ASME, EN). Hydrogen has substantial solubility in hot glycerin, resulting in false, non-conservative measurements that underestimate actual diffusible hydrogen by 30% to 60%.

Consumable Conditioning & Storage Protocols

SMAW Basic Electrodes (E7018, E8018): Supplied in hermetically sealed metal containers. Once opened, electrodes must be stored in holding ovens maintained at 120°C to 150°C (250°F to 300°F) . Maximum atmospheric exposure before re-baking is 4 hours (or 9 hours for moisture-resistant designators like E7018R / E7018-H4R). Contaminated or exposed electrodes must be reconditioned by baking at 370°C to 430°C (700°F to 800°F) for a minimum of 2 hours.

SAW Fluxes: Highly hygroscopic agglomerated fluxes must be kept in heated hoppers (100°C to 150°C) and re-baked at 300°C to 350°C if exposed to ambient moisture.