Study guide
11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation
Key Takeaways Explain This Topic AI
To prevent solidification cracking in ferritic steels, the Manganese-to-Sulfur ratio (Mn/S) must be maintained above 25-30, combined with low phosphorus and sulfur limits (P + S <= 0.015%), convex bead contours, and controlled heat input.
Lamellar tearing is a step-like cracking phenomenon beneath heavy-section T- and corner joints caused by through-thickness (Z-direction) tensile contraction stresses acting across flattened Type II manganese sulfide inclusions; it is mitigated using Z-grade steels (ASTM A770 Z25/Z35), buttering, and joint redesign.
Lamellar tearing is caused by through-thickness strain acting on planar non-metallic inclusions, so the primary cure is joint redesign rather than a change of consumable.
Buttering the plate face with low-strength ductile weld metal absorbs through-thickness strain before the restrained joint is completed.
Z-quality steel is specified by guaranteed through-thickness reduction of area, which is the direct measure of resistance to lamellar tearing.
Last updated: September 2026
- Engineering Mitigation of Lamellar Tearing
- 1. Material Specification: "Z-Grade" Steels (ASTM A770 / EN 10164)
Standard tensile tests measure mechanical properties in the longitudinal (rolling) or transverse directions. Due to inclusion flattening, short-transverse (through-thickness) ductility is dramatically inferior. To guarantee resistance to lamellar tearing, engineers specify Z-direction quality steels evaluated via ASTM A770 / A770M (Through-Thickness Tension Testing):
Z-Grade Designations:
Z15: Minimum average through-thickness reduction of area (ZRA) >= 15%.
Z25: Minimum average ZRA >= 25% (Standard for critical offshore and seismic joints).
Z35: Minimum average ZRA >= 35% (Severe restraint, extreme heavy plate applications).
Clean Steel Metallurgy: Achieving Z25/Z35 properties requires:
Vacuum degassing to eliminate dissolved gases.
Ultra-low sulfur refining ([S] <= 0.005%, frequently <= 0.002%).
Calcium Treatment (Inclusion Shape Control): Injecting calcium-silicon (Ca-Si) wire into the ladle converts elongated MnS into hard, non-deformable spherical calcium sulfides/calcium aluminates (CaS * Al2O3). These spherical inclusions retain their shape during rolling, eliminating planar stringers and raising Z-direction reduction of area above 40%.
2. Buttering (Buffer Layer Technique)
When Z-grade plate is unavailable, a ductile buffer layer (buttering) can be deposited directly on the surface of the susceptible plate before joint assembly:
Deposit 2 to 3 layers (6 to 10 mm thickness) of a low-strength, high-ductility weld metal (e.g., ER70S-3, E7018-1, or austenitic nickel alloy).
Grind the buttering flat, then fit up the mating member and weld the full joint entirely to the buttered layer.
The buttering layer spreads transverse contraction strains across a broader volume and isolates the susceptible inclusion-rich plate core from high peak welding stresses.
3. Joint Redesign to Avoid Z-Direction Stresses JOINT REDESIGN TO PREVENT LAMELLAR TEARING
- SUSCEPTIBLE DESIGN (POOR) MITIGATED DESIGN (EXCELLENT)
- (Tensile Shrinkage Acts Across (Shrinkage Vector Transferred
- Plate Through-Thickness) to In-Plane Shear or Forging)
- | | | |
- | | | |
- | | | |
- +-----+---+-----+ +-----+---+-----+
- | | | | | | | |
- | / \ | | / \ |
- | / \ | | / \ |
- ==+==+=========+==+=== ==+==+=========+==+===
- || | Tear! | || || | Machined | | ||
- || +---------+ || || | Corner / | | ||
- || Rolled Plate || || | Forging | | ||
- ====================== ======================
Move bevel preparations from the attached through-plate to the cross-member so that weld fusion crosses the plate surface at an oblique angle.
Replace welded T-joints with rolled or forged transition sections (e.g., cast steel nodes in offshore jackets) that place weld seams outside the Z-direction stress zone.
Use recessed corner joints where the vertical plate extends past the corner, converting through-thickness tension into in-plane longitudinal shear.
- Worked Numerical Example: Hot Cracking Susceptibility & Aspect Ratio Evaluation
- Problem Statement
A mechanized Submerged Arc Welding (SAW) procedure is being developed to weld a longitudinal seam in a heavy structural box girder fabricated from carbon steel plate. Metallurgical analysis of the test weld reveals the following fusion zone chemical composition (weight percent):
- Carbon (C): 0.16%
- Manganese (Mn): 0.75%
- Silicon (Si): 0.35%
- Sulfur (S): 0.030%
- Phosphorus (P): 0.025%
- Niobium (Nb): 0.035%
The initial welding procedure operates at 32 V, 750 A, and 450 mm/min travel speed (7.5 mm/s), producing a macro-etched cross-section with:
- Bead Width (W): 14.0 mm
- Bead Depth (D): 17.5 mm
Engineering Tasks:
Calculate the Manganese-to-Sulfur ratio (Mn/S) and evaluate compliance with crack-prevention criteria.
Calculate the Unit of Cracking Susceptibility (UCS) for carbon-manganese weld metals using the established UK Welding Institute formulation: UCS = 230*C + 190*S + 75*P + 45*Nb - 12.3*Si - 5.4*Mn - 1.0 where values > 20 indicate severe solidification cracking susceptibility, 10 to 20 indicates borderline risk, and < 10 indicates high resistance.
Calculate the depth-to-width aspect ratio (D/W) of the initial weld bead and evaluate crack risk.
Recommend optimized welding parameter adjustments (voltage, current, travel speed) to achieve a crack-resistant bead profile (D/W <= 0.70) without sacrificing required weld throat penetration.
- Step-by-Step Solution
- Step 1: Calculate Mn/S Ratio Mn / S = 0.75% / 0.030% = 25.0
Evaluation: The ratio equals 25.0, which is at the absolute lower threshold of the acceptable 25 to 30 boundary. Given the high sulfur concentration (0.030%) and presence of phosphorus (0.025%), the alloy lacks an adequate safety margin to suppress low-melting Fe-FeS films under rigid restraint.
Step 2: Calculate Unit of Cracking Susceptibility (UCS) UCS = 230*(0.16) + 190*(0.030) + 75*(0.025) + 45*(0.035) - 12.3*(0.35) - 5.4*(0.75) - 1.0
- UCS = 36.8 + 5.70 + 1.875 + 1.575 - 4.305 - 4.05 - 1.0
- UCS = 45.95 - 9.355 = 36.595 approx 36.6
Evaluation: Because UCS = 36.6 significantly exceeds the critical threshold of 20.0, this weld metal chemistry is classified as exceptionally prone to solidification cracking .
Step 3: Calculate Bead Aspect Ratio (D/W) D / W = 17.5 mm / 14.0 mm = 1.25
Evaluation: The depth-to-width ratio D/W = 1.25 > 1.0 produces a deep, narrow weld pool. Solidifying columnar dendrites meet at an abrupt 90° angle at the joint centerline. Because UCS = 36.6 and D/W = 1.25, centerline hot cracking is virtually guaranteed under transverse restraint.
Step 4: Process Parameter Optimization To eliminate centerline cracking:
Increase Arc Voltage (from 32 V to 36 V): Arc length expands, widening the arc cone and broadening the bead width (W) from 14 mm to 22 mm.
Reduce Welding Current (from 750 A to 600 A): Decreases arc force and plasma jet momentum, reducing penetration depth (D) from 17.5 mm to 12.0 mm.
Resulting Aspect Ratio: D_new / W_new = 12.0 mm / 22.0 mm = 0.545 <= 0.70
Consumable Substitution: Switch to a higher-manganese, basic-flux combination (e.g., Lincoln 880M flux with Lincolnweld L-61 wire) to elevate weld metal manganese to 1.20% and reduce sulfur to <= 0.010%, driving Mn/S > 120 and reducing UCS < 10.
- Real-World Engineering Scenarios & Exam Pitfalls
- Industrial Scenario: Lamellar Tearing in an Offshore Platform Jacket Node
During the fabrication of a critical node connection for an offshore oil platform, 75 mm thick ASTM A572 Grade 50 rolled plates were welded into a heavy cruciform joint using full-penetration submerged arc welds with heavy joint restraint. Radiographic testing (RT) showed no fusion defects. However, subsequent straight-beam ultrasonic testing (UT) revealed intermittent planar discontinuities 5 to 8 mm below the plate surface, extending several hundred millimeters parallel to the weld fusion line.
Failure Analysis:
Core trepan samples exhibited classic step-like "terrace-and-wall" lamellar tearing.
Mill test records revealed the plate was standard structural grade with sulfur at 0.028% and no through-thickness reduction of area guarantee. Heavy planar Type II MnS inclusions were verified via scanning electron microscopy.
Remediation:
The defective plates were gouged out completely.
Replacement plates were ordered to ASTM A770 Z35 specifications ([S] <= 0.002%, calcium treated for inclusion globularity, through-thickness reduction of area > 35%).
Before making the CJP welds, an 8 mm three-pass buttering layer of ductile E7018-1 weld metal was deposited across the plate face to absorb residual transverse shrinkage strain.
Common Exam Traps
Exam Trap 1: Confusing Solidification Cracking with Lamellar Tearing Solidification cracking occurs in the weld metal along the centerline or between dendrites at temperatures near the alloy solidus (> 1000°C). Lamellar tearing occurs in the base metal plate beneath the weld along inclusion stringers parallel to the rolling plane at temperatures below 200°C.
Exam Trap 2: Increasing Heat Input to "Soften" Hot Cracks A dangerous misconception is that increasing heat input prevents hot cracking by retarding the cooling rate (as it does for cold cracking). For hot cracking, increasing heat input worsens cracking susceptibility ! Higher heat input expands the volume of the molten pool, broadens the Brittle Temperature Range (BTR), coarsens dendrites, increases microsegregation, and increases total contraction strain.
Exam Trap 3: The Directionality of Lamellar Tearing Stresses Lamellar tearing is driven solely by tensile strains acting in the Z-direction (through-thickness / short-transverse) perpendicular to the plate surface. It cannot be caused by longitudinal stresses running parallel to the plate rolling direction.