Study guide
11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention
Key Takeaways Explain This Topic AI
Preheat suppresses HICC by retarding the cooling rate through the 800°C to 500°C transformation window (delta t_8/5) to prevent hard martensite formation and by accelerating the solid-state effusion of diffusible hydrogen prior to cooling below 100°C.
Dehydrogenation Heat Treatment (DHT / post-heating) at 200°C to 300°C (400°F to 600°F) immediately following welding exponentially increases hydrogen diffusivity, safely outgassing hydrogen before the joint cools to room-temperature embrittlement ranges.
Post-heating holds a weld at a moderate temperature immediately after welding to let hydrogen diffuse out, and it is not the same operation as stress-relieving post-weld heat treatment.
Hydrogen cracking is delayed, so a weld that passes immediate inspection can crack hours or days later, which is why code hold times before inspection exist.
Removing any one of the four necessary conditions prevents cold cracking, and hydrogen level is usually the cheapest one to control.
Last updated: September 2026
- Preheat, Interpass, and Post-Heating Engineering Calculations
- Physical Mechanisms of Preheat
Preheat alters the welding thermal cycle through two distinct physical mechanisms:
Cooling Rate Retardation: Reduces the cooling rate through the critical austenite decomposition window (800°C to 500°C, denoted delta t_8/5): delta t_8/5 is proportional to: Q_net / [2 * pi * k * (T_interpass - T_0)] Extending delta t_8/5 promotes the transformation of austenite into benign, ductile ferrite-pearlite or upper bainite rather than hard, brittle martensite.
Hydrogen Effusion Acceleration: Extends the residence time between 300°C and 100°C, allowing mobile hydrogen atoms to diffuse out of the fusion zone and HAZ into the atmosphere before the steel cools to ambient temperatures where brittle cleavage occurs.
Preheat Calculation Frameworks
AWS D1.1 Annex H (Method A - Susceptibility Index): Categorizes base metals into Susceptibility Groups (I, II, III) based on composition, combines this with Diffusible Hydrogen Level (H1, H2, H3), and cross-references joint restraint thickness to dictate minimum preheat and interpass temperatures.
AWS D1.1 Annex H (Method B - Hardness Control Method): Uses Pcm to limit peak HAZ hardness below a specified maximum (HV_max <= 350 to 400 HV) based on critical cooling time: T_preheat = 1600 * Pcm - 280 (in °C)
EN 1011-2 / BS 5135 Method: Uses combined thickness d_c (sum of all plate thicknesses meeting at the joint line), heat input Q (kJ/mm), carbon equivalent CET, and hydrogen scale to extract preheat from standardized nomograms: CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40
Dehydrogenation Heat Treatment (DHT / Hydrogen Bakeout)
If a thick, highly restrained weld cannot be maintained at preheat temperature until non-destructive examination or full post-weld heat treatment (PWHT), a Dehydrogenation Heat Treatment (DHT) must be applied immediately upon arc extinction:
Parameters: Maintain the joint at 200°C to 300°C (400°F to 600°F) for a minimum soak time of 1 to 4 hours (typically 1 hour per 25 mm of joint thickness) prior to cooling below 100°C.
Diffusion Kinetics: The diffusion coefficient of hydrogen in ferritic iron follows the Arrhenius relationship: D_H = D_0 * exp(-Q_d / (R * T)) At 250°C, D_H is approximately 1.5 x 10^-5 cm^2/s, which is more than two orders of magnitude faster than at room temperature (20°C, D_H approx 1.2 x 10^-7 cm^2/s). The characteristic diffusion distance x approx 2 * sqrt(D_H * t) ensures that diffusible hydrogen effuses out of the joint before brittle room-temperature conditions are reached.
- Worked Numerical Example: Carbon Equivalency & Preheat Evaluation
- Problem Statement
A welding engineer is qualifying a welding procedure specification (WPS) for a critical structural offshore column connection. The joint is a complete-joint-penetration (CJP) double-V groove butt weld joining 50.0 mm thick plates of thermo-mechanically controlled processed (TMCP) structural steel. The certified mill test report (CMTR) reveals the following ladle chemical composition (all values in weight percent):
- Carbon (C): 0.09%
- Manganese (Mn): 1.45%
- Silicon (Si): 0.28%
- Chromium (Cr): 0.06%
- Molybdenum (Mo): 0.18%
- Nickel (Ni): 0.35%
- Copper (Cu): 0.22%
- Vanadium (V): 0.04%
- Boron (B): 0.0012%
- Niobium (Nb): 0.03%
- Phosphorus (P): 0.010%
- Sulfur (S): 0.003%
Calculations Required:
Calculate the International Institute of Welding Carbon Equivalent (CE_IIW).
Calculate the Ito-Bessyo Cracking Parameter (Pcm).
Determine which parameter (CE_IIW or Pcm) metallurgically governs this steel and justify your selection.
Using the empirical Ito-Bessyo minimum preheat formulation for thick, highly restrained joints: T_p (°C) = 1440 * P_c - 392 where P_c = Pcm + [H_diff]/60 + t/600 , evaluate T_p for:
Condition 1: Shielded Metal Arc Welding (SMAW) using improperly stored basic electrodes with H_diff = 12 mL/100g.
Condition 2: Flux-Cored Arc Welding (FCAW-G) using certified H4 consumables with H_diff = 3.5 mL/100g.
Calculate the DHT soak duration at 250°C required for hydrogen to diffuse an effective diffusion distance x = 25 mm (2.5 cm), given D_H(250°C) = 1.6 x 10^-5 cm^2/s.
- Step-by-Step Solution
- Step 1: Calculate CE_IIW CE_IIW = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
- CE_IIW = 0.09 + 1.45/6 + (0.06 + 0.18 + 0.04)/5 + (0.35 + 0.22)/15
- CE_IIW = 0.09 + 0.2417 + 0.28/5 + 0.57/15
- CE_IIW = 0.09 + 0.2417 + 0.0560 + 0.0380 = 0.4257%
- Step 2: Calculate Pcm Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5*B
- Pcm = 0.09 + 0.28/30 + (1.45 + 0.22 + 0.06)/20 + 0.35/60 + 0.18/15 + 0.04/10 + 5*(0.0012)
- Pcm = 0.09 + 0.00933 + 1.73/20 + 0.00583 + 0.0120 + 0.0040 + 0.0060
- Pcm = 0.09 + 0.00933 + 0.0865 + 0.00583 + 0.0120 + 0.0040 + 0.0060 = 0.2137%
Step 3: Metallurgical Parameter Selection The carbon concentration of this steel is C = 0.09%, which is substantially below the 0.18% threshold. Applying CE_IIW to low-carbon microalloyed/TMCP steels significantly overestimates the hardenability contribution of carbon and assigns excessive weight to alloying elements like manganese. Therefore, Pcm = 0.214% is the correct governing parameter for this steel.
Step 4: Calculate Minimum Preheat Temperature (T_p) Base plate thickness t = 50 mm. The thickness restraint term is: t / 600 = 50 / 600 = 0.0833
Condition 1: High Hydrogen (H_diff = 12 mL/100g) P_c1 = 0.2137 + 12/60 + 0.0833 = 0.2137 + 0.2000 + 0.0833 = 0.4970
T_p1 = 1440 * (0.4970) - 392 = 715.7 - 392 = 323.7°C approx 325°C (617°F)
Engineering Assessment: Requiring a 325°C preheat is excessively high, commercially impractical, and risks degrading the fine-grained TMCP microstructure through over-tempering.
Condition 2: Certified Low Hydrogen (H_diff = 3.5 mL/100g) P_c2 = 0.2137 + 3.5/60 + 0.0833 = 0.2137 + 0.0583 + 0.0833 = 0.3553
T_p2 = 1440 * (0.3553) - 392 = 511.6 - 392 = 119.6°C approx 120°C (248°F)
Engineering Assessment: By switching from non-controlled electrodes to certified H4 consumables, the minimum required preheat drops by over 200°C (from 325°C down to 120°C), demonstrating the critical impact of diffusible hydrogen control on fabrication economics and joint integrity.
Step 5: Calculate Dehydrogenation Post-Heat Soak Time Using the diffusion approximation x = 2 * sqrt(D_H * t) : t = x^2 / (4 * D_H) = (2.5 cm)^2 / [4 * (1.6 x 10^-5 cm^2/s)] = 6.25 / (6.4 x 10^-5) = 97,656 seconds
t = 97,656 / 3600 approx 27.1 hours (for single-surface effusion)
In standard industrial practice where hydrogen diffuses symmetrically across both top and bottom surfaces (maximum diffusion path length to nearest surface = t/2 = 25 mm = 1.25 cm): t_sym = (1.25 cm)^2 / [4 * (1.6 x 10^-5 cm^2/s)] = 1.5625 / (6.4 x 10^-5) = 24,414 s approx 6.78 hours
Conclusion: Specifying an immediate post-heat soak (DHT) of 250°C for 4 to 6 hours reduces the residual diffusible hydrogen concentration in the mid-thickness below the critical cracking threshold (< 1.0 mL/100g).
- Real-World Engineering Scenarios & Exam Pitfalls
- Industrial Scenario: Delayed Toe Cracking in Heavy Mining Shovel Booms
A heavy equipment manufacturer fabricated mining excavator booms using 65 mm thick ASTM A514 Grade B (690 MPa minimum yield strength) quenched and tempered plates. Multipass flux-cored arc welding (FCAW-G) was performed with a preheat of 110°C. Visual and magnetic particle testing (MT) conducted 2 hours after weld completion showed complete compliance. However, after full structural blast cleaning and painting 72 hours later, 100% shear toe cracking was observed running parallel to the fusion boundary across multiple structural diaphragms.
Failure Investigation & Root Cause:
NDE was conducted prematurely. For high-strength Q&T steels, AWS D1.1 Clause 8 mandates an inspection hold period of at least 48 hours post-weld.
The FCAW wire coils were left mounted on wire feeders inside the unheated shop over a humid weekend, absorbing moisture into the seam and flux core, driving diffusible hydrogen levels from an initial H4 (3.2 mL/100g) to > 14 mL/100g.
The preheat temperature of 110°C was inadequate for the high weld restraint and elevated hydrogen level.
Corrective Action: The fabricator instituted climate-controlled wire storage cabinets, increased preheat to 175°C, mandated an immediate dehydrogenation bakeout at 230°C for 2 hours post-weld, and enforced a strict 48-hour hold before final MT and ultrasonic examination.
Common Exam Traps
Exam Trap 1: Misapplying IIW CE to Modern Low-Carbon TMCP Steels Certification exam questions frequently present a steel with carbon content between 0.05% and 0.12% and ask which formula to use for preheat determination. Do not use CE_IIW for steels with carbon < 0.18%. CE_IIW was calibrated on 1940s-era normalized C-Mn steels; it grossly overestimates the preheat required for modern microalloyed steels. You must select the Ito-Bessyo Pcm formula.
Exam Trap 2: Preheat Only Retards Martensite Formation A widespread misconception is that preheating only serves to slow the cooling rate to avoid martensite. In high-strength steels, preheat's equally vital role is accelerating hydrogen effusion . At 150°C to 200°C, the diffusion rate of hydrogen is hundreds of times faster than at room temperature, allowing hydrogen to safely escape before the steel transforms to martensite and reaches room-temperature embrittlement ranges.
Exam Trap 3: Timing of HICC Formation If an exam question asks when hydrogen-induced cold cracking initiates, never select "during solidification" or "immediately upon arc extinguishment." HICC is delayed cracking occurring between -100°C and +200°C, typically hours or days after the joint has reached ambient temperature.