Study guide
11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding
Key Takeaways Explain This Topic AI
Aluminum welding metallurgy is dominated by its tenacious, refractory surface oxide (Al2O3, melting point 2050°C vs. Al 660°C), requiring AC GTAW cathodic cleaning where the DCEP half-cycle removes the dielectric oxide via ion bombardment.
A steep, 20-fold plunge in hydrogen solubility during aluminum solidification (0.70 mL/100g liquid to 0.036 mL/100g solid) makes hydrogen the sole cause of porosity in aluminum welds, requiring stringent hydrocarbon and moisture cleanliness.
Selection between ER4043 (Al-Si) and ER5356 (Al-Mg) filler metals is governed by base alloy chemistry, crack sensitivity curves, post-weld anodizing color match, ductility requirements, and service temperatures (<65°C to avoid Mg2Al3 stress corrosion cracking).
Titanium and reactive alloys absorb interstitial embrittling gases (O, N, H) above 400°C, mandating high-purity inert shielding (Ar 99.999%), trailing shields, backing purges (<50 ppm O2), and strict color inspection criteria.
Last updated: September 2026
11.4 Non-Ferrous Alloys: Aluminum, Titanium & Nickel Superalloys
Quick Answer: Welding non-ferrous engineering alloys requires overcoming extreme chemical reactivity, refractory surface films, and complex precipitation kinetics. Aluminum alloys feature a persistent refractory oxide film (Al2O3, melting point 2050°C vs. aluminum substrate at 660°C) that requires cathodic cleaning via alternating current (AC GTAW) or pulsed GMAW, alongside strict moisture control to prevent gas porosity caused by a > 20-fold drop in hydrogen solubility upon solidification. Heat-treatable alloys like 6061-T6 suffer severe HAZ softening due to beta-double-prime (Mg2Si) dissolution and coarsening. Titanium alloys (CP-Ti, Ti-6Al-4V) react voraciously with oxygen, nitrogen, and hydrogen at T > 400°C, mandating trailing shields and root backing purges (< 50 ppm O2) with weld acceptance verified by surface discoloration (silver/straw vs. rejectable blue/grey/white oxide). Nickel superalloys divide into solid-solution grades (Inconel 625, Hastelloy C-276) and precipitation-hardenable grades (Inconel 718, X-750); alloys with high aluminum and titanium ([Al] + [Ti] > 3.0% to 4.0%) are prone to strain-age cracking during post-weld heat treatment due to rapid gamma-prime (Ni3(Al,Ti)) precipitation.
- Aluminum Alloys: Metallurgy, Oxide Dynamics & Porosity
- Classification & Heat Treatability
Series Primary Alloying Element Strengthening Mechanism Typical Weldability Rating Common Structural Applications
1xxx Pure Aluminum (>= 99.0%) Strain hardening (non-heat-treatable) Excellent; low strength Electrical bus bars, chemical tanks
2xxx Copper (Cu) Precipitation hardening (heat-treatable) Poor (2024 crack-prone) to Fair (2219 highly weldable) Aerospace fuselage, cryogenic rocket tanks
3xxx Manganese (Mn) Solid solution / strain hardening Excellent; easily welded HVAC, heat exchangers, architectural sheet
4xxx Silicon (Si) Non-heat-treatable (some PH) Excellent; primarily filler metal (ER4043) Brazing sheet, welding filler rods
5xxx Magnesium (Mg) Solid solution / strain hardening Excellent; high joint efficiency Shipbuilding, pressure vessels, armor plate
6xxx Magnesium & Silicon (Mg-Si) Precipitation hardening (Mg2Si) Excellent with filler; crack-sensitive autogenous Structural frames, extrusion, bridge girders
7xxx Zinc & Magnesium (Zn-Mg) Precipitation hardening (MgZn2) Poor (7075 non-weldable) to Good (7005, 7039) Aircraft frames, military bridge pontoons
The Refractory Oxide Film & AC Cathodic Cleaning
All aluminum alloys are encapsulated by a naturally forming, thermodynamically stable dielectric film of aluminum oxide (Al2O3):
Melting Point Disparity: Aluminum oxide melts at 2050°C (3722°F) , whereas the underlying aluminum substrate melts at 660°C (1220°F) .
Density Disparity: Solid Al2O3 has a density of 3.95 g/cm^3, which is significantly heavier than molten aluminum (2.38 g/cm^3). If not removed, the oxide skins do not melt; they crumble, sink into the pool, and become jagged planar oxide inclusions (entrainment defects). AC GTAW CATHODIC CLEANING DYNAMICS
- ELECTRODE POSITIVE (DCEP / EP) ELECTRODE NEGATIVE (DCEN / EN)
- [ Cathodic Cleaning Mode ] [ Deep Penetration Mode ]
- Tungsten (-) Tungsten (-)
- | |
- v (Electrons) v (Electrons)
- ~~~~~~~~~~~~~ ~~~~~~~~~~~~~
- ^ ^ ^ ^ | | | |
- | | | | (Argon Ions) v v v v
- +---+---+---+ +---+---+---+
- | Base Metal| (Positive) | Base Metal| (Negative)
- +-----------+ +-----------+
- Heavy Ar+ ions blast surface; Electrons bombard workpiece;
dielectric oxide blasted away! transfers 70% heat for deep penetration.
In Alternating Current Gas Tungsten Arc Welding (AC GTAW):
Electrode Positive (DCEP / EP) Half-Cycle (Cathodic Cleaning): The workpiece acts as the cathode. Heavy, positively charged argon ions (Ar+) are accelerated across the cathode fall voltage into the workpiece surface. This physical ion bombardment blasts the brittle, dielectric Al2O3 film off the plate surface (cathodic sputtering / etching).
Electrode Negative (DCEN / EN) Half-Cycle (Heating & Penetration): Electrons boil off the thermionic tungsten cathode and bombard the plate, depositing thermal energy to achieve deep penetration while protecting the tungsten from overheating.
Modern Inverter Waveform Balance: Inverter power supplies allow independent adjustment of the EN balance (typically set between 65% and 75% EN ). This maximizes weld penetration and narrows the bead profile while retaining sufficient EP duration (25% to 35%) to clean the surface oxide.
Hydrogen Porosity Mechanism
Unlike steel, where porosity can result from nitrogen, carbon monoxide, or hydrogen, hydrogen is the sole cause of porosity in aluminum welds :
Solubility Drop: Molten aluminum at its melting point (660°C) dissolves up to 0.70 mL of hydrogen per 100 grams of metal. Upon phase transformation to solid aluminum, hydrogen solubility plummets to 0.036 mL / 100g —a 20-fold reduction in solubility !
Bubble Trapping: As dendrites advance, rejected hydrogen supersaturates the terminal liquid. If the cooling rate prevents bubbles from nucleating and floating to the pool surface (governed by Stokes' law), spherical gas porosity becomes permanently entrapped.
Moisture Control: The primary hydrogen source is hydrated aluminum oxide (Al2O3 * 3H2O) and hydrocarbon grease on wire/plate surfaces. Welding wire must be stored in dry, heated environments, and base plates must be degreased with solvent and stainless-steel wire-brushed immediately before welding. HYDROGEN SOLUBILITY IN ALUMINUM
- Solubility (mL H2 / 100g Al)
- |
- 0.80 | /--- Molten Liquid Phase
- 0.70 | / (High Solubility: ~0.70 mL/100g)
- 0.60 | /
- 0.50 | /
- 0.40 | /
- 0.30 | /
0.20 | / <--- 20x Precipitous Solubility Drop!
0.10 | / Drives Intense Hydrogen Porosity!
- 0.00 +--------------+-----+-----------------------------------
- 0 660°C T (Temperature)
- (Solidus)
- Solid Phase: 0.036 mL/100g
- Filler Metal Selection: ER4043 vs. ER5356
Al-Mg-Si alloys (e.g., 6061) exhibit extreme hot cracking susceptibility when welded autogenously (without filler), because their nominal composition (~1.0% Mg2Si) sits precisely atop the peak of the crack sensitivity curve. Adding filler metal shifts the fusion zone composition into crack-resistant regimes.
Engineering Property ER4043 (Al - 5.0% Si) ER5356 (Al - 5.0% Mg)
Solidification Range Narrow; lower melting point (574°C to 632°C) Broader; higher melting point (571°C to 635°C)
Weld Fluidity & Wetting Exceptional; smooth bead ripple, easy operation Moderate; more sluggish, higher arc spatter in GMAW
Crack Resistance High (shifts pool into hyper-eutectic regime) High (dilutes magnesium past crack peak)
Shear & Tensile Strength Lower (186 MPa typical fillet shear) Significantly higher (230 MPa typical fillet shear)
- Ductility & Toughness Moderate elongation (8% to 12%) High elongation (15% to 25%); superior impact toughness
- Anodizing Color Match POOR (Turns Dark Grey / Black) EXCELLENT (Matches base metal silver-bright)
- High-Temp Service (> 65°C) Permissible up to 150°C PROHIBITED if Mg > 3.0% (SCC risk from beta-phase)
- High-Magnesium Base Metals DO NOT USE on 5083, 5456 (brittle Mg2Si) Standard selection for 5xxx series
- HAZ Softening in 6061-T6
Alloy 6061-T6 achieves its high base-metal yield strength (~275 MPa / 40 ksi) via fine, coherent needle-like beta-double-prime (Mg2Si) precipitates produced by artificial aging (160°C to 180°C). The welding thermal cycle inevitably degrades this microstructure in the HAZ:
Partial Dissolution Zone (T_peak > 400°C): Beta-double-prime precipitates dissolve back into solid solution. Upon cooling, insufficient aging kinetics leave the zone in a soft, naturally aged state.
Over-Aging Zone (200°C <= T_peak <= 380°C): The fine beta-double-prime needles coarsen into rod-shaped beta-prime and incoherent equilibrium beta (Mg2Si) platelets, eliminating precipitation strengthening.
Mechanical Consequence: The as-welded tensile strength drops from 310 MPa down to the minimum code-specified as-welded tensile strength of 165 MPa (24 ksi) (AWS D1.2 Table 3.2). This strength loss cannot be restored without a complete post-weld solution heat treatment, water quench, and artificial aging (re-T6).
Titanium & Reactive Metals Welding Metallurgy
Titanium (CP-Ti, Ti-6Al-4V) and reactive alloys (zirconium, niobium, tantalum) are exceptional chemical "getters." At temperatures exceeding 400°C (750°F) , titanium reacts voraciously with atmospheric gases:
Oxygen and Nitrogen Absorption: Dissolve interstitially into the hexagonal close-packed (HCP) alpha lattice, severely expanding lattice constants, impeding dislocation motion, and destroying fracture toughness and bend ductility.
Hydrogen Absorption: Precipitates as brittle titanium hydrides (TiH2), inducing delayed hydride embrittlement and catastrophic subcritical crack growth.
Carbon Contamination: Reacts to form brittle intergranular titanium carbides (TiC). TITANIUM SHIELDING GAS ARCHITECTURE
- Torch Cup (Primary Shield)
- | |
- | GTAW |
- | Torch |
- +-------+
- | Gas |
- | Lens |---- Primary Argon Envelope
- Trailing Shield +-------+
- +------------------+ |
- | Porous Sintered | v Arc
- | Diffuser Plate |====> [ Molten Pool ]
- +------------------+ +----------------+
- | | Cooling HAZ | Solidified Bead
- v +----------------+ (T > 400°C)
- Argon Flood Blanket |
- Protects cooling weld v
- until T < 400°C! [ Backing Gas Purge Chamber (< 50 ppm O2) ]
- Comprehensive Shielding Architecture
Welding titanium outside of a sealed, inert glovebox requires a three-tiered shielding system using ultra-high-purity argon (99.999%, dew point <= -60°C / -76°F):
Primary Torch Shielding: Large-diameter ceramic nozzle equipped with a porous sintered stainless-steel gas lens to establish laminar, non-turbulent shielding flow.
Secondary Trailing Shield: A secondary auxiliary chamber attached directly behind the welding torch. As the torch advances, the trailing shield floods the cooling solidified weld metal and adjacent HAZ with inert gas until surface temperatures drop below 400°C (750°F) .
Backside Purging: Full root purge using purge dams, copper backing bars with gas diffusers, or complete chamber enclosure. The oxygen concentration in the backing exit gas must be monitored with an optical oxygen analyzer and verified below 50 ppm (preferably < 20 ppm) before arc ignition.
Surface Discoloration & Inspection Criteria (AWS G2.4 / AWS D17.1)
The interference color of the surface oxide film on a completed titanium weld provides a direct indicator of atmospheric contamination level:
- Surface Oxide Color Contamination Severity Underlying Metallurgy Code Acceptance (AWS D17.1 Class A)
- Bright Silver None Pristine inert shielding; zero gas pickup Fully Acceptable
Light Straw / Gold Very Light Superficial surface oxide formed at lower temperatures (< 450°C) Acceptable ; surface oxide easily removed
Dark Straw / Amber Light Slight interstitial diffusion into outer surface Acceptable for non-critical ; strip before multi-pass
Peacock / Blue / Purple Moderate Interstitial gas absorption during cooling (450°C to 650°C) UNACCEPTABLE ; causes significant loss of ductility
Grey / Dull Grey Severe Deep oxygen/nitrogen diffusion; hardened alpha case REJECTED ; brittle; must be mechanically excavated
White Loose Powder / Chalky Catastrophic Gross atmospheric exposure; thick porous oxide scale REJECTED; SCRAP COMPONENT ; severe embrittlement