11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization
Key Takeaways Explain This Topic AI
The five stainless steel families (austenitic, ferritic, martensitic, duplex, and precipitation-hardening) exhibit fundamentally distinct weldabilities governed by crystal structure, phase stability, and thermal expansion.
The WRC-1992 diagram is the modern engineering standard for predicting delta ferrite in austenitic and duplex stainless steel weld metals, employing refined Cr_eq and Ni_eq formulas that explicitly account for nitrogen and copper while eliminating silicon and manganese distortions.
Sensitization results from chromium carbide (Cr23C6) precipitation along austenite grain boundaries during exposure to 500°C to 850°C, creating a chromium-depleted zone (<12% Cr) susceptible to intergranular corrosion; it is mitigated via low-carbon 'L' grades (C <= 0.03%), stabilization with Ti/Nb, or full solution annealing.
Last updated: September 2026
11.3 Stainless Steels: Schaeffler/WRC-1992 Diagrams, Sensitization & Duplex
Quick Answer: Welding stainless steels requires precise thermodynamic control of phase balance, solid-state precipitation, and solidification modes. Austenitic grades (e.g., 304L, 316L) require a controlled delta ferrite content of 3 to 8 Ferrite Number (FN) to guarantee primary ferrite (FA) solidification, preventing solidification cracking while avoiding brittle sigma phase formation at high temperatures or loss of cryogenic impact toughness. Modern constitution prediction relies on the WRC-1992 diagram , which accurately incorporates nitrogen and copper equivalents. Sensitization —intergranular corrosion caused by Cr23C6 carbide precipitation and adjacent chromium depletion (< 12% Cr) in the 500°C to 850°C window—is eliminated using low-carbon "L" grades (C <= 0.030%) or stabilized grades (321 with Ti, 347 with Nb). Duplex stainless steels (2205, 2507) require strict heat input management (0.5 to 2.5 kJ/mm), nickel-overalloyed filler metals, and nitrogen-supplemented shielding to maintain a 40% to 60% austenite-ferrite balance.
Stainless Steel Alloy Families & Welding Metallurgy
Family Crystal Structure Representative Alloys Magnetic? Primary Welding Challenges & Metallurgical Phenomena
Austenitic FCC (Face-Centered Cubic) AISI 304/304L, 316/316L, 310, 347 Non-magnetic Solidification hot cracking if fully austenitic (0 FN); HAZ sensitization in high-carbon grades; high thermal expansion (50% greater than carbon steel) causing severe angular distortion.
Ferritic BCC (Body-Centered Cubic) AISI 409, 430, 444 Strongly magnetic Rapid high-temperature grain coarsening (T > 950°C) in HAZ causing irreversible loss of toughness; cannot be grain-refined by heat treatment; 475°C embrittlement.
Martensitic BCT (Body-Centered Tetragonal) AISI 410, 420, 440C Strongly magnetic Extreme hardenability upon air cooling; high susceptibility to hydrogen-induced cold cracking (HICC); requires mandatory preheat (200°C to 300°C) and immediate post-weld tempering (650°C to 750°C).
Duplex / Super-Duplex Dual-Phase (~50% gamma + 50% delta) 2205 (UNS S32205), 2507 (UNS S32750) Magnetic Preserving phase balance; preventing excessive ferrite in HAZ due to rapid cooling; avoiding precipitation of brittle intermetallics (sigma, chi, chromium nitrides) during slow cooling.
Precipitation-Hardening (PH) Martensitic / Semiaustenitic 17-4PH (UNS S17400), 15-5PH Magnetic Matching base metal strength via post-weld aging (480°C to 620°C); avoiding over-aging in HAZ; managing high residual stresses in restrained joints.
Constitutional Diagrams: Schaeffler, DeLong & WRC-1992
To predict the as-solidified weld metal microstructure resulting from base metal dilution and filler metal alloying, welding engineers rely on constitutional diagrams that plot Chromium Equivalent (ferrite stabilizers) versus Nickel Equivalent (austenite stabilizers). EVOLUTION OF CONSTITUTIONAL DIAGRAMS
- SCHAEFFLER (1949) DeLONG (1973) WRC-1992 (Modern)
- Historic baseline - Added Nitrogen (30*N) - AWS A5.4 / ASME IX Standard
- Cr_eq: Cr+Mo+1.5Si+0.5Nb - Up to 18 FN - Cr_eq: Cr + Mo + 0.7Nb
- Ni_eq: Ni+30C+0.5Mn - Underestimates high FN - Ni_eq: Ni + 35C + 20N + 0.25Cu
- Ignores Nitrogen - Predicts Ferrite Number - Eliminates Si and Mn errors
- Mathematical Formulations
- Schaeffler Diagram (1949): Cr_eq, Schaeffler = Cr + Mo + 1.5*Si + 0.5*Nb
- Ni_eq, Schaeffler = Ni + 30*C + 0.5*Mn
Limitations: Developed before the significant role of nitrogen in stainless steel was understood. Completely ignores nitrogen, leading to large errors in modern nitrogen-strengthened or argon-shielded welds.
- DeLong Diagram (1973): Cr_eq, DeLong = Cr + Mo + 1.5*Si + 0.5*Nb
- Ni_eq, DeLong = Ni + 30*C + 30*N + 0.5*Mn
Advancement: Introduced nitrogen weighting (30 x N) and introduced the standardized magnetic Ferrite Number (FN) scale up to 18 FN.
WRC-1992 Diagram (Kotecki & Siewert - Current Industry Standard): Adopted by AWS A5.4, ASME Section III, and ASME Section IX as the authoritative reference diagram for weld metal constitution: Cr_eq, WRC-1992 = Cr + Mo + 0.7*Nb
Ni_eq, WRC-1992 = Ni + 35*C + 20*N + 0.25*Cu
Key Engineering Improvements:
Eliminates silicon (Si) and manganese (Mn) terms because extensive experimental data demonstrated their effects are negligible within normal commercial ranges (< 1% Si, < 2.5% Mn).
Corrects carbon potency from 30 to 35, and nitrogen potency from 30 to 20.
Incorporates copper (0.25 x Cu) as an austenite stabilizer.
Extends FN prediction reliably up to 100 FN , fully covering duplex and super-duplex stainless steels.
- Ferrite Number (FN) & Solidification Modes
- Ferrite Number vs. Percent Ferrite
Historically, ferrite was measured by metallographic point counting, which produced extreme inter-laboratory scatter (5% to 15% discrepancy on identical samples). To resolve this, AWS A4.2 and ISO 8249 established the Ferrite Number (FN) , an internationally calibrated magnetic measurement scale using instruments such as the Magne-Gage or Ferritescope. For standard austenitic steels below 10 FN, FN is roughly equal to volume percent ferrite (1 FN approx 1 vol%). Above 10 FN, the relationship becomes non-linear.
The Four Solidification Modes of Austenitic Welds
Solidification behavior is governed by the ratio of equivalents (Cr_eq / Ni_eq): SOLIDIFICATION MODES IN AUSTENITIC WELDS
- Mode A (Cr/Ni < 1.25) : L -> L + A -> A [HIGH CRACK RISK!]
- Mode AF (1.25 < Cr/Ni < 1.48): L -> L + A -> L + A + F -> A + F
- Mode FA (1.48 < Cr/Ni < 1.95): L -> L + F -> L + F + A -> F + A [CRACK-RESISTANT!]
- Mode F (Cr/Ni > 1.95) : L -> L + F -> F [HIGH FERRITE]
Mode A (Fully Austenitic): Liquid solidifies directly to primary austenite (L -> gamma). Low-melting impurities (S, P) are rejected into liquid films wetting the smooth, planar austenite boundaries. Severe risk of solidification cracking.
Mode AF (Primary Austenite with Interdendritic Ferrite): Austenite dendrites solidify first, with delta ferrite forming from terminal liquid at dendrite boundaries.
Mode FA (Primary Ferrite with Interdendritic Austenite - TARGET REGIME): Delta ferrite solidifies first as skeletal dendrites (L -> delta), followed by a peritectic-eutectic reaction where austenite nucleates and consumes liquid and ferrite (L + delta -> gamma). Solidification in FA mode provides two vital cracking defenses:
Impurity Solubility: The solubility of sulfur and phosphorus in delta ferrite is roughly 10 times higher than in austenite, sequestering S and P within solid solution.
Tortuous Grain Boundaries: The migrating phase transformation creates complex, jagged interphase boundaries that physically block crack propagation.
Mode F (Fully Ferritic): Primary ferrite solidifies (L -> delta) without peritectic transformation; cools with high residual ferrite.
Engineering Targets for Ferrite Number
General Fabrication (Crack Prevention): 3 to 8 FN (or 4 to 10 FN). Guarantees FA mode solidification without compromising mechanical properties.
Cryogenic Service (LNG, -196°C): Restrict to <= 3 to 5 FN . Body-centered cubic delta ferrite undergoes a ductile-to-brittle transition, degrading Charpy V-notch energy and lateral expansion at liquid nitrogen temperatures.
High-Temperature Service (> 550°C): Restrict to <= 8 to 10 FN . Prolonged exposure to elevated temperatures transforms delta ferrite into brittle sigma phase .
Urea / Highly Oxidizing Nitric Acid Service: Mandates 0 FN (Fully Austenitic) . Delta ferrite suffers preferential selective dissolution in concentrated nitric acid; requires specialized ultra-low S and P grades (e.g., 310L, 316L Modified).
- Sensitization & Intergranular Corrosion (IGC)
- Thermodynamics of Chromium Depletion
When austenitic stainless steels are heated into or slowly cooled through the critical temperature range of 500°C to 850°C (950°F to 1550°F) —such as in the weld Heat-Affected Zone—sensitization occurs: SENSITIZATION MICROSTRUCTURE
- [ Austenite Grain ] [ Austenite Grain ]
- (18% Cr) (18% Cr)
- \ /
- \ Chromium-Depleted Zone /
- \ (< 12% Cr) /
- v v
- |=====| |=====|
- | Cr | Cr23C6 Carbide | Cr |
- | Dep | Precipitates at | Dep |
- | Zone| Grain Boundary | Zone|
- |=====| |=====|
- Grain Boundary Interface
Kinetics: Carbon is a small interstitial atom with a high diffusion coefficient, while chromium is a large substitutional atom that diffuses much slower. Carbon diffuses rapidly from grain interiors to prior-austenite grain boundaries.
Carbide Precipitation: Carbon combines with chromium along the grain boundary to precipitate complex chromium carbides, predominantly Cr23C6 (or M23C6): 23 Cr + 6 C -> Cr23C6
Chromium-Depleted Zone: Because chromium diffusion is slow, the chromium extracted to form the carbide is drawn almost entirely from a thin layer (< 100 nm) immediately adjacent to the grain boundary. Matrix chromium concentration in this zone drops precipitously from the baseline 18% down to < 12% —falling below the critical threshold required to form a protective, passive chromium oxide (Cr2O3) film.
Galvanic Dissolution: When exposed to electrolyte environments (marine, chemical process, acid), the narrow chromium-depleted boundary behaves as a tiny active anode driven by the massive surrounding cathode of passive grain interiors, resulting in catastrophic intergranular corrosion (IGC) or intergranular stress corrosion cracking (IGSCC).
- Industrial Mitigation Strategies THE THREE SENSITIZATION DEFENSES
- |
- +--------------------------+--------------------------+
- | | |
- v v v
- [ Low-Carbon Grades ] [ Stabilized Grades ] [ Solution Annealing ]
- AISI 304L / 316L - AISI 321 (Ti >= 5*C) - 1050°C to 1150°C Soak
- C <= 0.030 wt% - AISI 347 (Nb >= 10*C) - Rapid Water Quench
- Starves carbide growth - Ties up carbon at >1000°C - Redissolves carbides
Low-Carbon "L" Grades (AISI 304L, 316L): Specifying maximum carbon <= 0.030% starves the carbide precipitation reaction. The "nose" of the Time-Temperature-Sensitization (TTS) curve is shifted from seconds to hours, allowing standard multi-pass welding without sensitization.
Stabilized Grades (AISI 321, 347): Incorporate strong carbide-forming elements:
Titanium (AISI 321): Requires Ti >= 5 x C. Forms titanium carbide (TiC) at temperatures > 1000°C, consuming carbon before chromium carbides can precipitate.
Niobium (AISI 347): Requires Nb >= 10 x C. Forms niobium carbide (NbC).
Knife-Line Attack (KLA): In narrow HAZ regions heated to > 1200°C, TiC and NbC dissolve. If subsequent passes reheat this zone to 500°C to 850°C, chromium carbides precipitate, creating a razor-thin band of attack. Mitigated via a post-weld stabilization heat treatment at 870°C to 900°C (1600°F to 1650°F) to redissolve Cr23C6 and re-precipitate stable TiC/NbC.
Full Solution Annealing: Heating the completed weldment to 1050°C to 1150°C , soaking to fully dissolve all carbides back into solid solution, followed by a rapid water quench past 500°C in seconds.