Study guide
12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols
Key Takeaways Explain This Topic AI
A sharp break in the arrow line explicitly points to the specific component in a groove weld that must receive edge beveling or J-preparation.
Joint architecture selection balances five fundamental geometries (butt, corner, T, lap, and edge) against Complete Joint Penetration (CJP) versus Partial Joint Penetration (PJP), where PJP introduces an intrinsic unfused root crack notch sensitive to cyclic fatigue.
Nondestructive examination symbols use the same reference-line grammar as weld symbols, with arrow side below the line and other side above.
Examination extent is shown as a length or percentage to the right of the method letters, and the number of examinations goes in parentheses in the tail.
A complete joint penetration groove weld develops the full base-metal section and is not sized by the designer, whereas a partial joint penetration weld has a designer-specified effective throat.
Last updated: September 2026
Standard Joint Architecture Selection
AWS defines five basic structural joint configurations. Sizing and selecting the proper architecture depends on the primary stress mode, accessibility, fabrication economics, and non-destructive examination (NDE) inspectability. BUTT JOINT CORNER JOINT T-JOINT
- [Member 1][Member 2] [Member 1] [Member 1]
- | | | | |
- +------+ +----+----+
- [Member 2] [Member 2]
- LAP JOINT EDGE JOINT
- [Member 1]====== [Member 1]|
- ======[Member 2] [Member 2]|
- Joint Architecture Engineering Comparison
Joint Type Primary Load Path Stress Concentration Points Edge Preparation Cost Primary NDE Method
Butt (B) Direct axial tension/compression; bending Minimal when CJP ground flush ( K t ≈ 1.0 K_t \approx 1.0 K t ≈ 1.0 ) High (beveling, planing, milling) Volumetric: RT (Radiography) or UT (Ultrasonic)
Corner (C) Bending moments; internal pressure High stress at interior corner root Moderate to High (single/double bevel) UT, MT (Magnetic Particle), or VT (Visual)
T-Joint (T) Transverse shear; axial tension/compression High notch effect at weld toes and root Low for fillet; High for deep bevel UT (for bevels), MT/PT (for fillets)
Lap (L) Longitudinal or transverse shear High eccentricity, peeling, secondary bending Zero edge prep (shear/flame cut) Visual (VT), MT, or PT (Liquid Penetrant)
Edge (E) Low shear; sealing; light structural Severe notch at root; cannot carry tension Zero (parallel plate edges) Visual (VT), PT
Complete Joint Penetration (CJP) vs. Partial Joint Penetration (PJP)
The choice between Complete Joint Penetration (CJP) and Partial Joint Penetration (PJP) represents one of the most critical structural and economic decisions in welding engineering. CJP GROOVE WELD PJP GROOVE WELD
(Full Cross-Section Fused) (Unwelded Root Land Remains)
- \ / \ /
- \ Sound Weld / \ Sound Weld /
- \ Metal / \ Metal /
- ================= -----------------
- | Unwelded Root | <-- Severe Notch
- ---------------- (Kt > 3.0)
- Comparative Engineering Mechanics
Complete Joint Penetration (CJP):
Definition: A groove weld in which weld metal extends completely through the joint thickness, fully fusing the base metal across the entire cross-section.
Mechanical Performance: When executed with matching filler metal, a CJP groove weld transmits the full static tensile, compressive, and shear capacity of the base metal. Its design strength is identical to that of the parent plate ( F allow = F base F_{\text{allow}} = F_{\text{base}} F allow = F base ).
Fatigue Resistance: Excellent. When weld reinforcement is ground flush with the plate surface and volumetric NDE confirms absence of planar flaws, a CJP butt joint achieves AISC Fatigue Category B .
Fabrication Cost: High. Requires precise fit-up, backing strips or back-gouging to sound metal (e.g., carbon arc gouging), and extensive volumetric non-destructive examination (UT/RT).
Partial Joint Penetration (PJP):
Definition: A groove weld in which weld metal does not extend through the joint thickness, leaving an un-welded root face or root land by design.
Mechanical Performance: The effective throat ( E E E ) is strictly less than the plate thickness ( t t t ). Capable of transmitting static compression and moderate static shear.
Fatigue Resistance: Extremely Poor. The unwelded root face constitutes an intrinsic, pre-existing sharp crack notch. Under cyclic axial tension or out-of-plane bending, high stress concentrations ( K t > 3.0 K_t > 3.0 K t > 3.0 ) trigger rapid fatigue crack propagation along the unwelded interface. Consequently, PJP groove welds are categorized under severe fatigue classes ( AISC Category C' or E ) and are strictly prohibited in cyclically loaded tensile tension connections.
Fabrication Cost: Low. Eliminates back-gouging, requires less filler metal (often 50% to 70% reduction in weld volume), and significantly lowers residual stresses and angular distortion.
Nondestructive Examination Symbols (AWS A2.4)
AWS B5.16 Clause 8.3.1 lists NDE symbols as a required Part 3 topic, and AWS A2.4 standardizes them in the same reference-line grammar as weld symbols — which is exactly why they are tested here alongside welding symbols.
Method Letter Designations
The examination method is given by standard letters placed on the reference line:
- Letter Method Letter Method
- VT Visual ET Eddy current
- PT Liquid penetrant AET Acoustic emission
- MT Magnetic particle LT Leak testing
- RT Radiographic NRT Neutron radiographic
- UT Ultrasonic PRT Proof testing
Combined methods are written with a plus sign (for example MT + UT ) when more than one method is required on the same joint.
Placement Grammar
The side conventions mirror the weld symbol exactly:
Below the reference line (arrow side): examine the arrow side of the joint.
Above the reference line (other side): examine the other side.
On both sides, or centred on the reference line with the line broken : examine from both sides.
Placing the letters centred on the reference line with no arrow-side/other-side distinction indicates the method may be applied from either side.
Additional elements:
Extent of examination is shown by the length dimension placed to the right of the method letters; with no dimension given, examination is full length.
Number of examinations is placed in parentheses in the tail — RT (4) calls for four radiographs.
Partial or spot examination is indicated by a percentage or a length, for example UT 20% or MT 6 .
The tail carries the governing specification, procedure or acceptance standard.
A radiation direction symbol with its angle may be added to fix the beam orientation for RT.
Combination Weld and NDE Symbols
The same reference line can carry both instructions: the weld symbol on one side and the examination symbol on the other. A single-V groove symbol below the line with RT above it specifies an arrow-side single-V groove weld that is to be radiographed from the other side.
Exam Trap: Reading the NDE side convention backwards. Arrow side is below the reference line for both weld symbols and examination symbols. Candidates who memorize "below equals arrow side" for welds but then invert it for NDE lose the point. The convention is identical; only the content of the symbol changes.
- Comprehensive Worked Engineering Example: Deciphering Complex Welding Callouts
- Problem Statement
A structural fabrication drawing specifies the following complex welding symbol on a heavy crane column-to-baseplate T-joint connecting a 36 mm 36\text{ mm} 36 mm thick ASTM A572 Gr 50 web to a 65 mm 65\text{ mm} 65 mm thick base plate: G
- (---)
- 16(20) 60°
- --/-----\----------(100% UT)-----> (Points to vertical web)
- \ /
- |> 12 100 - 250
(A field weld flag is present at the junction pointing away from the arrow, and a broken arrow line breaks downward, pointing directly at the 36 mm 36\text{ mm} 36 mm web plate).
Provide the complete engineering interpretation of this symbol, specifying: (a) which plate is beveled and what the preparation dimensions are, (b) the other-side weld details, (c) the finishing and inspection requirements, and (d) the location of fabrication.
- Step-by-Step Engineering Solution
- Step 1: Identify Arrow Break and Edge Preparation (Arrow Side)
The symbol on the bottom (Arrow Side) is a Single-Bevel Groove with a bevel angle and dimensions.
The arrow line is broken and points directly at the 36 mm 36\text{ mm} 36 mm vertical web. Therefore, the web plate must be beveled; the 65 mm 65\text{ mm} 65 mm base plate remains square.
The depth of bevel preparation is S = 16 mm S = 16\text{ mm} S = 16 mm .
The minimum required effective throat is E = 20 mm E = 20\text{ mm} E = 20 mm (the parenthesized dimension). Because E > S E > S E > S , the welding procedure must achieve 4 mm 4\text{ mm} 4 mm of deep penetration beyond the bevel root face.
The included groove angle is α = 60 ∘ \alpha = 60^\circ α = 6 0 ∘ .
Step 2: Identify Other-Side Weld Details
The symbol on top (Other Side) is a Fillet Weld .
The leg size is w = 12 mm w = 12\text{ mm} w = 12 mm (placed to the left of the fillet triangle).
The weld is an intermittent fillet weld: segment length L = 100 mm L = 100\text{ mm} L = 100 mm , center-to-center pitch P = 250 mm P = 250\text{ mm} P = 250 mm . The unwelded gap between segments is P − L = 250 − 100 = 150 mm P - L = 250 - 100 = 150\text{ mm} P − L = 250 − 100 = 150 mm .
Step 3: Finishing and Contour Requirements
Above the other-side fillet symbol sits a flush contour symbol --- topped by the finish designator G .
Interpretation: The 12 mm 12\text{ mm} 12 mm intermittent fillet welds on the other side must be ground flush with the base metal surface using mechanical grinding ( G G G ).
Step 4: Tail References and Fabrication Location
The field weld flag is attached to the reference line junction. Interpretation: This joint is a field weld to be erected and welded on site, not in the fabrication shop.
The tail contains the specification "100% UT". Interpretation: The entire length of the groove weld must undergo 100% Ultrasonic Testing in accordance with the governing structural code (AWS D1.1 Clause 8).
- Industrial Scenarios & Certified Welding Engineer Exam Pitfalls
- Real-World Field Disaster Scenario
During the erection of a seismic moment frame for a 40-story commercial tower, the fabricator misinterpreted an unbroken arrow line on a single-bevel groove joint between a 50 mm 50\text{ mm} 50 mm column flange and a 25 mm 25\text{ mm} 25 mm beam continuity doubler plate. The detailer failed to include a break in the arrow line, intending for the thinner doubler plate to be beveled. The shop beveled the 50 mm 50\text{ mm} 50 mm column flange instead. This mistake inverted the bevel volume, quadrupled the required weld metal from 4.2 kg/m 4.2\text{ kg/m} 4.2 kg/m to 16.8 kg/m 16.8\text{ kg/m} 16.8 kg/m , severely overheated the through-thickness Z-direction grain structure of the column, and caused catastrophic lamellar tearing directly beneath the fusion line during shop cooling. The column had to be scrapped, resulting in an eight-week project delay and $420,000 in replacement steel and ultrasonic testing costs.
Common Exam Traps
Exam Trap 1: Fillet Symbol Orientation In AWS A2.4, the perpendicular leg of the fillet right triangle must always be drawn on the left side , regardless of which direction the arrow points. Candidates who draw the perpendicular leg on the right side or mirror it based on arrow direction will lose full credit on Part 3 design questions.
Exam Trap 2: Length and Pitch Order ( L − P L - P L − P ) When sizing intermittent welds, length and pitch are separated by a hyphen to the right of the symbol: L − P L - P L − P . Pitch is never the clear distance between welds; it is always the center-to-center spacing! If an exam question specifies a 50 mm 50\text{ mm} 50 mm weld with an unwelded space of 100 mm 100\text{ mm} 100 mm , the pitch is P = 50 + 100 = 150 mm P = 50 + 100 = 150\text{ mm} P = 50 + 100 = 150 mm . The correct callout is 50 − 150 50 - 150 50 − 150 .
Exam Trap 3: Groove Depth ( S S S ) vs. Effective Throat ( E E E ) When a symbol reads 10 ( 12 ) 10(12) 10 ( 12 ) , 10 10 10 is the prepared depth of bevel ( S S S ), and ( 12 ) (12) ( 12 ) is the effective design throat ( E E E ). If only a single unparenthesized number appears (e.g., 10 10 10 ), then by definition S = E = 10 mm S = E = 10\text{ mm} S = E = 10 mm . If only a single parenthesized number appears (e.g., ( 12 ) (12) ( 12 ) ), the engineering drawing dictates the required effective throat, leaving the specific depth of preparation S S S and root gap to the fabricator's qualified WPS.