Study guide
12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test
Key Takeaways Explain This Topic AI
A stress gradient determines how much material sees near-peak stress, which is why a sharp notch in a thick section is more damaging than the same notch in a thin one.
The fillet weld break test is the only practical way to see the root of a fillet weld, which no surface method and no radiograph of a tee joint reveals reliably.
A fillet break specimen that bends flat without fracturing passes; the fracture-surface acceptance limits apply only if it actually breaks.
Plug and slot welds are sized on the nominal area of the hole or slot, not on the fillet-like fusion around its perimeter.
Last updated: September 2026
Plug and Slot Welds
Plug and slot welds transmit shear across overlapping plates by filling a circular hole or elongated slot with weld metal.
Structural Mechanics and Sizing Equations
Effective Shearing Area ( A w A_w A w ): Equal to the nominal area of the hole or slot in the plane of the faying surface: A w = π d 2 4 ( for circular plug welds ) A_w = \frac{\pi d^2}{4} \quad (\text{for circular plug welds}) A w = 4 π d 2 ( for circular plug welds ) A w = W ⋅ L − ( 1 − π / 4 ) W 2 ≈ W ⋅ L ( for slots with rounded ends ) A_w = W \cdot L - (1 - \pi/4) W^2 \approx W \cdot L \quad (\text{for slots with rounded ends}) A w = W ⋅ L − ( 1 − π /4 ) W 2 ≈ W ⋅ L ( for slots with rounded ends )
Design Shear Strength:
LRFD: ϕ R n = 0.75 × ( 0.60 F E X X ) A w = 0.45 F E X X A w \phi R_n = 0.75 \times (0.60 F_{EXX}) A_w = 0.45 F_{EXX} A_w ϕ R n = 0.75 × ( 0.60 F EXX ) A w = 0.45 F EXX A w
ASD: R n / Ω = 0.60 F E X X 2.00 A w = 0.30 F E X X A w R_n / \Omega = \frac{0.60 F_{EXX}}{2.00} A_w = 0.30 F_{EXX} A_w R n /Ω = 2.00 0.60 F EXX A w = 0.30 F EXX A w
Dimensional Limitations (AWS D1.1 Clause 4.10 & AISC J2.3):
Minimum hole diameter: d min = t + 8 mm d_{\min} = t + 8\text{ mm} d m i n = t + 8 mm ( t + 5 / 16 in t + 5/16\text{ in} t + 5/16 in ), where t t t is plate thickness.
Maximum hole diameter: d max = 2.25 t d_{\max} = 2.25 t d m a x = 2.25 t or d min + 3 mm d_{\min} + 3\text{ mm} d m i n + 3 mm .
Depth of fill: For plates t ≤ 16 mm t \le 16\text{ mm} t ≤ 16 mm ( 5 / 8 in 5/8\text{ in} 5/8 in ), depth of fill must equal plate thickness. For t > 16 mm t > 16\text{ mm} t > 16 mm , minimum depth of fill is t / 2 t/2 t /2 , but not less than 16 mm 16\text{ mm} 16 mm .
Stress Gradients Across Welded Sections
AWS B5.16 Clause 8.3.5 lists stress gradient alongside sectional properties and stress triaxiality. A stress gradient is the rate at which stress changes with position, d σ / d x d\sigma/dx d σ / d x , and welding engineers care about three distinct gradients:
Structural (bending) gradient. Pure axial load produces a uniform stress field with zero gradient. Bending produces a linear through-thickness gradient from tension at one surface to compression at the other, crossing zero at the neutral axis. A weld placed near the neutral axis of a beam sees almost no bending stress; the same weld moved to the flange sees the peak. This is why flange-to-web welds in plate girders are sized for horizontal shear flow while the flange butt splice is sized for the full bending stress.
Geometric (notch) gradient. A weld toe, reinforcement, undercut or backing bar produces a steep local gradient over a distance of a fraction of a millimetre. The peak stress is K t K_t K t times nominal, but it decays rapidly into the plate. A steep gradient means only a small highly stressed volume , so a sharp notch is much less damaging in a small part than the same K t K_t K t in a thick section — the mechanism behind the thickness-correction factors in fatigue codes.
Residual stress gradient. Longitudinal residual stress peaks near yield at the weld centreline and falls, often reversing into compression, within a few plate thicknesses. Superimposed on applied stress, this shifts the effective mean stress at the toe and is why as-welded fatigue curves are treated as mean-stress independent.
The engineering significance of a gradient is that fracture and fatigue respond to the stressed volume, not just the peak value . A shallow gradient exposes a large volume of material to near-peak stress, giving a high probability of finding a critical defect; a steep gradient shelters the bulk. This is the physical basis of the "highly stressed volume" and weakest-link statistical arguments used to explain why thick sections behave worse than thin sections at identical nominal stress. Relative stress gradient: χ = 1 σ max ⋅ d σ d x ∣ surface \text{Relative stress gradient: } \chi = \frac{1}{\sigma_{\max}}\cdot\frac{d\sigma}{dx}\bigg|_{\text{surface}} Relative stress gradient: χ = σ m a x 1 ⋅ d x d σ surface
A high χ \chi χ (steep gradient, small stressed volume) correlates with higher apparent fatigue strength; a low χ \chi χ approaches the uniform-stress worst case.
The Fillet Weld Break Test
Clause 8.3.5 also names the fillet break test (influence of second phase and porosity) . It is the cheapest destructive check on a fillet weld and appears in both AWS D1.1 welder qualification and WPS qualification for fillet welds.
Method. A fillet weld is deposited on a T-joint test coupon. The specimen is loaded so the fillet is forced to fracture through its throat — typically by pressing or hammering the stem of the tee over until the weld breaks or the stem bends flat against the plate. The fracture surface is then examined, because it exposes the root of the fillet, which no surface method and no radiograph of a tee joint can see reliably.
What the fracture face reveals.
- Feature on the fracture surface What it proves
- Bright, fully fused root Correct root penetration and arc placement
- Dark unfused notch at the root Incomplete fusion — the most common fillet defect and an automatic reject
- Rounded voids Porosity from moisture, mill scale, oil or lost shielding
- Dull, glassy, angular inclusions Entrapped slag or second-phase non-metallic inclusions
- Flat, faceted, low-energy fracture Brittle weld metal or excessive hardness
Acceptance. The current edition of AWS D1.1 accepts a fillet weld break specimen that either does not fracture at all, or — if it does fracture — shows complete fusion to the root of the joint with no single inclusion or pore greater than 3 / 32 in 3/32\text{ in} 3/32 in ( 2.5 mm 2.5\text{ mm} 2.5 mm ) in its greatest dimension, and with the sum of the greatest dimensions of all inclusions and porosity not exceeding 3 / 8 in 3/8\text{ in} 3/8 in ( 10 mm 10\text{ mm} 10 mm ) in the 6 in 6\text{ in} 6 in ( 150 mm 150\text{ mm} 150 mm ) specimen. Always read the acceptance table in the edition invoked by the contract, since the dimensional limits are edition-specific.
Exam Trap: "A bent-but-unbroken specimen fails the fillet break test." The opposite is true. A specimen that bends flat without fracturing demonstrates that the weld is stronger and more ductile than the base plate stem, and it passes. The fracture surface criteria apply only when fracture actually occurs.
- Comprehensive Worked Engineering Example: Sizing a Tension Lap Joint
- Problem Statement
A structural tension member consisting of an ASTM A572 Gr 50 flat bar ( F y = 345 MPa F_y = 345\text{ MPa} F y = 345 MPa , F u = 450 MPa F_u = 450\text{ MPa} F u = 450 MPa , thickness t = 12 mm t = 12\text{ mm} t = 12 mm , width b = 180 mm b = 180\text{ mm} b = 180 mm ) is spliced to a gusset plate using a lap joint. The joint is subjected to a service dead load P D = 140 kN P_D = 140\text{ kN} P D = 140 kN and service live load P L = 260 kN P_L = 260\text{ kN} P L = 260 kN .
Welding is executed using the GMAW process with matching AWS A5.18 ER70S-6 filler metal ( F E X X = 70 ksi ≈ 485 MPa F_{EXX} = 70\text{ ksi} \approx 485\text{ MPa} F EXX = 70 ksi ≈ 485 MPa ). Fillet weld leg size is specified as w = 8.0 mm w = 8.0\text{ mm} w = 8.0 mm .
Calculate the required length of longitudinal fillet welds using: (a) LRFD methodology, and (b) ASD methodology. Then, (c) verify the connection capacity if a transverse fillet weld of length b = 180 mm b = 180\text{ mm} b = 180 mm is added across the end of the plate under LRFD. +----------------------------------+
- | |========== Longitudinal Weld (L)
- | A572 Gr 50 Plate |
- Pu <--| t = 12 mm, b = 180 mm |
- | |========== Longitudinal Weld (L)
- +----------------------------------+
- | Transverse Weld (b = 180 mm)
- Step-by-Step Engineering Solution
- Step 1: Compute Factored and Service Loads
LRFD Factored Load ( P u P_u P u ): P u = 1.2 P D + 1.6 P L = 1.2 ( 140 kN ) + 1.6 ( 260 kN ) = 168 + 416 = 584 kN = 584 , 000 N P_u = 1.2 P_D + 1.6 P_L = 1.2(140\text{ kN}) + 1.6(260\text{ kN}) = 168 + 416 = 584\text{ kN} = 584,000\text{ N} P u = 1.2 P D + 1.6 P L = 1.2 ( 140 kN ) + 1.6 ( 260 kN ) = 168 + 416 = 584 kN = 584 , 000 N
ASD Service Load ( P a P_a P a ): P a = P D + P L = 140 kN + 260 kN = 400 kN = 400 , 000 N P_a = P_D + P_L = 140\text{ kN} + 260\text{ kN} = 400\text{ kN} = 400,000\text{ N} P a = P D + P L = 140 kN + 260 kN = 400 kN = 400 , 000 N
Step 2: Effective Throat and Unit Weld Capacities
Equal leg w = 8.0 mm ⟹ t e = 0.7071 w = 0.7071 ( 8.0 ) = 5.657 mm w = 8.0\text{ mm} \implies t_e = 0.7071 w = 0.7071(8.0) = 5.657\text{ mm} w = 8.0 mm ⟹ t e = 0.7071 w = 0.7071 ( 8.0 ) = 5.657 mm .
Nominal shear stress for longitudinal weld ( θ = 0 ∘ \theta = 0^\circ θ = 0 ∘ ): F n w = 0.60 F E X X = 0.60 × 485 MPa = 291.0 MPa = 291.0 N/mm 2 F_{nw} = 0.60 F_{EXX} = 0.60 \times 485\text{ MPa} = 291.0\text{ MPa} = 291.0\text{ N/mm}^2 F n w = 0.60 F EXX = 0.60 × 485 MPa = 291.0 MPa = 291.0 N/mm 2
Step 3: Required Longitudinal Weld Length under LRFD
Design shear strength per linear mm of longitudinal weld ( ϕ = 0.75 \phi = 0.75 ϕ = 0.75 ): ϕ q n = ϕ F n w t e = 0.75 × 291.0 N/mm 2 × 5.657 mm = 1234.6 N/mm = 1.2346 kN/mm \phi q_{n} = \phi F_{nw} t_e = 0.75 \times 291.0\text{ N/mm}^2 \times 5.657\text{ mm} = 1234.6\text{ N/mm} = 1.2346\text{ kN/mm} ϕ q n = ϕ F n w t e = 0.75 × 291.0 N/mm 2 × 5.657 mm = 1234.6 N/mm = 1.2346 kN/mm
Total required weld length for two longitudinal welds: L total = P u ϕ q n = 584.0 kN 1.2346 kN/mm = 473.0 mm L_{\text{total}} = \frac{P_u}{\phi q_n} = \frac{584.0\text{ kN}}{1.2346\text{ kN/mm}} = 473.0\text{ mm} L total = ϕ q n P u = 1.2346 kN/mm 584.0 kN = 473.0 mm
Length per side: L side = 473.0 / 2 = 236.5 mm ⟹ L_{\text{side}} = 473.0 / 2 = 236.5\text{ mm} \implies L side = 473.0/2 = 236.5 mm ⟹ Specify 240 mm 240\text{ mm} 240 mm per side .
Step 4: Required Longitudinal Weld Length under ASD
Allowable shear strength per linear mm of longitudinal weld ( Ω = 2.00 \Omega = 2.00 Ω = 2.00 ): q allow = F n w t e Ω = 291.0 × 5.657 2.00 = 823.1 N/mm = 0.8231 kN/mm q_{\text{allow}} = \frac{F_{nw} t_e}{\Omega} = \frac{291.0 \times 5.657}{2.00} = 823.1\text{ N/mm} = 0.8231\text{ kN/mm} q allow = Ω F n w t e = 2.00 291.0 × 5.657 = 823.1 N/mm = 0.8231 kN/mm
Total required weld length: L total = P a q allow = 400.0 kN 0.8231 kN/mm = 485.9 mm L_{\text{total}} = \frac{P_a}{q_{\text{allow}}} = \frac{400.0\text{ kN}}{0.8231\text{ kN/mm}} = 485.9\text{ mm} L total = q allow P a = 0.8231 kN/mm 400.0 kN = 485.9 mm
Length per side: L side = 485.9 / 2 = 243.0 mm ⟹ L_{\text{side}} = 485.9 / 2 = 243.0\text{ mm} \implies L side = 485.9/2 = 243.0 mm ⟹ Specify 245 mm 245\text{ mm} 245 mm per side .
Step 5: Incorporating a Transverse End Fillet under LRFD (AISC J2.4)
Sizing a transverse weld across plate width L trans = b = 180 mm L_{\text{trans}} = b = 180\text{ mm} L trans = b = 180 mm :
For transverse weld ( θ = 90 ∘ \theta = 90^\circ θ = 9 0 ∘ ): F n w t = 1.50 × ( 0.60 F E X X ) = 1.50 × 291.0 = 436.5 MPa F_{nwt} = 1.50 \times (0.60 F_{EXX}) = 1.50 \times 291.0 = 436.5\text{ MPa} F n wt = 1.50 × ( 0.60 F EXX ) = 1.50 × 291.0 = 436.5 MPa ϕ R n w t = ϕ F n w t t e L trans = 0.75 × 436.5 N/mm 2 × 5.657 mm × 180 mm = 333 , 354 N = 333.35 kN \phi R_{nwt} = \phi F_{nwt} t_e L_{\text{trans}} = 0.75 \times 436.5\text{ N/mm}^2 \times 5.657\text{ mm} \times 180\text{ mm} = 333,354\text{ N} = 333.35\text{ kN} ϕ R n wt = ϕ F n wt t e L trans = 0.75 × 436.5 N/mm 2 × 5.657 mm × 180 mm = 333 , 354 N = 333.35 kN
Using AISC Equation J2-10b to find required longitudinal length ( L long L_{\text{long}} L long ): ϕ R n = 0.85 ϕ R n w l + 1.5 ϕ R n w t ⟹ P u = 0.85 ( ϕ q n ⋅ L long ) + ϕ R n w t \phi R_n = 0.85 \phi R_{nwl} + 1.5 \phi R_{nwt} \implies P_u = 0.85 (\phi q_n \cdot L_{\text{long}}) + \phi R_{nwt} ϕ R n = 0.85 ϕ R n wl + 1.5 ϕ R n wt ⟹ P u = 0.85 ( ϕ q n ⋅ L long ) + ϕ R n wt 584.0 kN = 0.85 ( 1.2346 ⋅ L long ) + 333.35 584.0\text{ kN} = 0.85(1.2346 \cdot L_{\text{long}}) + 333.35 584.0 kN = 0.85 ( 1.2346 ⋅ L long ) + 333.35 0.85 ( 1.2346 ) L long = 584.0 − 333.35 = 250.65 kN 0.85(1.2346) L_{\text{long}} = 584.0 - 333.35 = 250.65\text{ kN} 0.85 ( 1.2346 ) L long = 584.0 − 333.35 = 250.65 kN 1.0494 L long = 250.65 ⟹ L long = 238.8 mm 1.0494 L_{\text{long}} = 250.65 \implies L_{\text{long}} = 238.8\text{ mm} 1.0494 L long = 250.65 ⟹ L long = 238.8 mm
Length per longitudinal side: 238.8 / 2 = 119.4 mm ⟹ 238.8 / 2 = 119.4\text{ mm} \implies 238.8/2 = 119.4 mm ⟹ Specify 120 mm 120\text{ mm} 120 mm per side .
Result: Adding the 180 mm 180\text{ mm} 180 mm transverse weld cuts the required longitudinal weld length in half (from 240 mm 240\text{ mm} 240 mm to 120 mm 120\text{ mm} 120 mm per side), drastically compacting the joint overlap length.
- Industrial Scenarios & Certified Welding Engineer Exam Pitfalls
- Real-World Field Disaster Scenario
A mobile crane outrigger support arm fabricated from ASTM A514 high-yield steel ( F y = 690 MPa F_y = 690\text{ MPa} F y = 690 MPa , 100 ksi 100\text{ ksi} 100 ksi ) experienced catastrophic shear fracture during a maximum-rated lift. The structural engineer specified an overmatched electrode (AWS A5.5 E11018-M) for all fillet welds, reasoning that higher strength equaled higher safety. During full-load lifting, while the weld metal remained elastic, the concentrated shear strain localized abruptly into the narrow, un-tempered martensitic Heat-Affected Zone (HAZ) of the A514 base plate. Because the overmatched weld provided zero plastic strain relaxation, a cleavage shear crack initiated at the weld root and ripped through the outrigger box section, dropping the crane boom onto an active highway. Subsequent failure analysis demonstrated that had an undermatched E7018 filler metal been used, the weld throat would have yielded plastically by 0.8 mm 0.8\text{ mm} 0.8 mm , redistributing stress safely across the entire outrigger assembly without cracking.
Common Exam Traps
Exam Trap 1: Forgetting the 3 mm (1/8 in) Deduction on 45° PJP Welds When an exam problem specifies a Partial Joint Penetration (PJP) groove weld prepared at a 45 ∘ 45^\circ 4 5 ∘ included angle welded with SMAW or FCAW-S without backing, candidates almost invariably take E = S E = S E = S . You must subtract 3 mm 3\text{ mm} 3 mm ( 1 / 8 in 1/8\text{ in} 1/8 in ) from the depth of preparation: E = S − 3 mm E = S - 3\text{ mm} E = S − 3 mm . If the preparation depth is 12 mm 12\text{ mm} 12 mm , the design effective throat is only 9 mm 9\text{ mm} 9 mm .
Exam Trap 2: Direct Addition of Longitudinal and Transverse Capacities When calculating the combined capacity of a weld group containing both longitudinal and transverse welds, you cannot simply compute R n = 1.0 R n w l + 1.5 R n w t R_n = 1.0 R_{nwl} + 1.5 R_{nwt} R n = 1.0 R n wl + 1.5 R n wt . Transverse welds reach their peak strength and fracture at deformations of only ≈ 0.05 w \approx 0.05 w ≈ 0.05 w , well before longitudinal welds develop their full yield strength. You must evaluate both AISC Equation J2-10a ( R n = R n w l + R n w t R_n = R_{nwl} + R_{nwt} R n = R n wl + R n wt ) and Equation J2-10b ( R n = 0.85 R n w l + 1.5 R n w t R_n = 0.85 R_{nwl} + 1.5 R_{nwt} R n = 0.85 R n wl + 1.5 R n wt ) and select the higher value.
Exam Trap 3: Overlooking Base Metal Shear Rupture Along Fusion Boundary Sizing the weld throat is only half the problem. When thin plates ( t < 1.414 w t < 1.414 w t < 1.414 w ) are joined by large fillet welds, the base metal along the fusion boundary will shear rupture before the weld throat yields. Always verify that base metal allowable shear ( 0.40 F y t L 0.40 F_y t L 0.40 F y t L or 0.30 F u t L 0.30 F_u t L 0.30 F u t L ) exceeds the applied load.