Study guide
13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity
Key Takeaways Explain This Topic AI
Industrial radiography relies on differential radiation absorption governed by the Beer-Lambert attenuation law (I = I0 e^(-μt)); radioisotopes (Iridium-192, Cobalt-60, Selenium-75) offer portable monoenergetic gamma emission, while X-ray machines provide controllable continuous Bremsstrahlung spectra.
Radiographic film optical density (D = log10(I0 / It)) must be maintained within tight code windows: 1.8 to 4.0 for X-ray radiographs and 2.0 to 4.0 for gamma radiographs per ASME Section V and AWS D1.1, with density across the weld area not varying beyond -15% to +30% of the IQI body density.
Image Quality Indicators (IQIs) verify radiographic sensitivity; standard inspection demands 2-2T sensitivity for hole-type plaques (resolving the 2T hole on a plaque whose thickness is 2% of specimen thickness) or equivalent essential wire resolution under ASTM E747 / ISO 19232.
Last updated: September 2026
13.2 Volumetric Radiography (RT): Geometric Unsharpness & Film/Digital Imaging
Quick Answer: Industrial Radiographic Testing (RT) evaluates internal volumetric soundess by directing ionizing radiation through a weldment onto photographic film or a digital detector. Differential absorption follows the Beer-Lambert law ( I = I 0 e − μ t I = I_0 e^{-\mu t} I = I 0 e − μ t ). Image penumbra is controlled by the geometric unsharpness formula ( U g = f ⋅ d D U_g = \frac{f \cdot d}{D} U g = D f ⋅ d ), where code limits mandate U g ≤ 0.020 in U_g \le 0.020\text{ in} U g ≤ 0.020 in ( 0.51 mm 0.51\text{ mm} 0.51 mm ) for steel under 2 in 2\text{ in} 2 in ( 50 mm 50\text{ mm} 50 mm ). Optical density must fall between 1.8 and 4.0 1.8\text{ and }4.0 1.8 and 4.0 for X-ray and 2.0 and 4.0 2.0\text{ and }4.0 2.0 and 4.0 for gamma rays. Image Quality Indicators (hole-type plaques or wire IQIs) verify standard 2-2T sensitivity . While volumetric flaws (porosity, slag, tungsten) are readily identified, planar lack of fusion and cracks require beam alignment within ± 5 ∘ to 10 ∘ \pm 5^\circ\text{ to }10^\circ ± 5 ∘ to 1 0 ∘ of the flaw plane.
1. Physics of Industrial Radiography: Sources, Spectra & Attenuation
Radiographic examination relies on high-energy electromagnetic photons possessing wavelengths between 10 − 4 and 10 nm 10^{-4}\text{ and }10\text{ nm} 1 0 − 4 and 10 nm . As radiation penetrates steel, photons undergo absorption and scattering primarily through the Photoelectric Effect (predominant at low energies, < 100 keV < 100\text{ keV} < 100 keV ), Compton Scattering (predominant across industrial welding energies, 100 keV to 5 MeV 100\text{ keV to }5\text{ MeV} 100 keV to 5 MeV ), and Pair Production (occurring at high energies, > 1.022 MeV > 1.022\text{ MeV} > 1.022 MeV ). VOLUMETRIC RADIOGRAPHIC EXPOSURE GEOMETRY
- Source / Focal Spot (f)
- +-----+
- | * |
- +--+--+
- | \
- | \
- Source-to-Object | \
- Distance (SOD = D) | \
- | \
- V V
- ====================[===WELD===]==================== Plate
- ====================================================
- Object-to-Film (d) | |
- -------------------+--------+----------------------
- [==FILM==]
- Source-to-Film Distance
- (SFD = D + d)
- X-Ray Machines vs. Radioisotope Gamma Sources
Industrial X-Ray Generators: X-rays are produced when high-velocity electrons accelerated across an electrical potential ( k V p kV_p k V p ) strike a heavy metal target (tungsten). The deceleration produces a continuous Bremsstrahlung spectrum superimposed with sharp characteristic emission lines. The tube voltage ( k V p kV_p k V p ) dictates photon energy (penetrating power), while tube current ( m A mA m A ) and exposure time ( s s s ) dictate total photon flux (intensity).
Gamma-Ray Radioisotopes: Gamma rays originate from the spontaneous nuclear decay of unstable radioactive isotopes, yielding discrete, monochromatic photon energy lines.
Radiation Source Physical Form & Half-Life ( t 1 / 2 t_{1/2} t 1/2 ) Principal Photon Energies Steel Thickness Inspection Range Half-Value Layer (HVL) in Steel
Iridium-192 ( 192 Ir ^{192}\text{Ir} 192 Ir ) Metallic pellet; t 1 / 2 = 73.83 days t_{1/2} = 73.83\text{ days} t 1/2 = 73.83 days Multi-line spectrum: 0.21 to 0.61 MeV 0.21\text{ to }0.61\text{ MeV} 0.21 to 0.61 MeV (average ≈ 0.38 MeV \approx 0.38\text{ MeV} ≈ 0.38 MeV ) 0.25 to 2.5 in 0.25\text{ to }2.5\text{ in} 0.25 to 2.5 in ( 6.4 to 65 mm 6.4\text{ to }65\text{ mm} 6.4 to 65 mm ) ≈ 0.50 in \approx 0.50\text{ in} ≈ 0.50 in ( 12.7 mm 12.7\text{ mm} 12.7 mm )
Cobalt-60 ( 60 Co ^{60}\text{Co} 60 Co ) Metallic pellet; t 1 / 2 = 5.27 years t_{1/2} = 5.27\text{ years} t 1/2 = 5.27 years Two distinct lines: 1.17 MeV 1.17\text{ MeV} 1.17 MeV and 1.33 MeV 1.33\text{ MeV} 1.33 MeV (average 1.25 MeV 1.25\text{ MeV} 1.25 MeV ) 1.5 to 7.0 in 1.5\text{ to }7.0\text{ in} 1.5 to 7.0 in ( 38 to 175 mm 38\text{ to }175\text{ mm} 38 to 175 mm ) ≈ 0.85 in \approx 0.85\text{ in} ≈ 0.85 in ( 21.6 mm 21.6\text{ mm} 21.6 mm )
Selenium-75 ( 75 Se ^{75}\text{Se} 75 Se ) Solid salt pellet; t 1 / 2 = 119.8 days t_{1/2} = 119.8\text{ days} t 1/2 = 119.8 days Multi-line: 0.066 to 0.40 MeV 0.066\text{ to }0.40\text{ MeV} 0.066 to 0.40 MeV (average ≈ 0.22 MeV \approx 0.22\text{ MeV} ≈ 0.22 MeV ) 0.15 to 1.0 in 0.15\text{ to }1.0\text{ in} 0.15 to 1.0 in ( 4.0 to 25 mm 4.0\text{ to }25\text{ mm} 4.0 to 25 mm ) ≈ 0.30 in \approx 0.30\text{ in} ≈ 0.30 in ( 7.6 mm 7.6\text{ mm} 7.6 mm )
Industrial X-Ray (300 kVp) Vacuum tube; continuous electrical operation Continuous spectrum up to 300 keV 300\text{ keV} 300 keV peak Up to 2.0 in 2.0\text{ in} 2.0 in ( 50 mm 50\text{ mm} 50 mm ) Variable with filtration; ≈ 0.25 in \approx 0.25\text{ in} ≈ 0.25 in ( 6.4 mm 6.4\text{ mm} 6.4 mm )
Attenuation Mathematics: Beer-Lambert Law, HVL & TVL
Radiation passing through matter attenuates exponentially according to the Beer-Lambert Law : I = I 0 e − μ t I = I_0 e^{-\mu t} I = I 0 e − μ t
where I 0 I_0 I 0 is the incident beam intensity, I I I is the transmitted beam intensity, μ \mu μ is the linear attenuation coefficient of the material ( cm − 1 \text{cm}^{-1} cm − 1 or in − 1 \text{in}^{-1} in − 1 ), and t t t is the material thickness.
Half-Value Layer (HVL): The thickness of absorber required to reduce the beam intensity to exactly 50 % 50\% 50% ( 1 / 2 1/2 1/2 ) of its initial value: I I 0 = 0.5 = e − μ ⋅ H V L ⟹ H V L = ln ( 2 ) μ = 0.69315 μ \frac{I}{I_0} = 0.5 = e^{-\mu \cdot HVL} \implies HVL = \frac{\ln(2)}{\mu} = \frac{0.69315}{\mu} I 0 I = 0.5 = e − μ ⋅ H V L ⟹ H V L = μ ln ( 2 ) = μ 0.69315
Tenth-Value Layer (TVL): The thickness of absorber required to attenuate the beam intensity to 10 % 10\% 10% ( 1 / 10 1/10 1/10 ): T V L = ln ( 10 ) μ = 2.3026 μ ≈ 3.32 × H V L TVL = \frac{\ln(10)}{\mu} = \frac{2.3026}{\mu} \approx 3.32 \times HVL T V L = μ ln ( 10 ) = μ 2.3026 ≈ 3.32 × H V L
2. Geometric Unsharpness ( U g U_g U g ) Mechanics & Code Limits
Because radiation sources possess finite physical dimensions (focal spot width f f f in an X-ray tube, or the physical diameter of a radioactive isotope pellet), rays originate from multiple points across the source face. This geometric dispersion casts a blurred shadow boundary—known as the geometric penumbra or geometric unsharpness ( U g U_g U g ) —along every feature edge on the film. GEOMETRIC UNSHARPNESS MECHANICS
- Source Diameter / Spot (f)
- |<- f ->|
- +-------+
- / \
- / \
- / \
- Source-to-Object / \
- Distance (SOD = D)/ \
- / \
- / \
- / Object / Defect \
- -------------------+------[=======]----------+--------------------
- Weldment Plate |<--w-->|
- Object-to-Film (d) / \
- ------------------+-------------------+---------------------------
- |<--Ug->| |<--Ug->|
- Blur Full Shadow Blur
- Film Plane / Detector
- Governing Formula
From similar triangles across the optical projection: U g = f ⋅ d D U_g = \frac{f \cdot d}{D} U g = D f ⋅ d
where:
- U g U_g U g = Geometric unsharpness (penumbra width on film)
- f f f = Source size (effective focal spot dimension of X-ray tube or active diameter of radioisotope capsule)
d d d = Object-to-film distance (OFD, distance from the source-side surface of the weldment to the recording media)
D D D = Source-to-object distance (SOD, distance from radiation source to the source-side surface of the weldment)
Note: Source-to-Film Distance is S F D = D + d = S O D + O F D SFD = D + d = SOD + OFD SF D = D + d = SO D + OF D .
To minimize geometric unsharpness ( U g U_g U g ), the welding engineer must:
Select the smallest practical source/focal spot size ( f f f ).
Minimize object-to-film distance ( d d d ) by placing film cassettes in direct contact with the weld root/face.
Maximize source-to-object distance ( D D D ), balancing penumbra reduction against the Inverse Square Law ( I ∝ 1 / S F D 2 I \propto 1 / SFD^2 I ∝ 1/ SF D 2 ), which increases exposure time quadratically.
Code Acceptance Limits for Geometric Unsharpness
ASME BPVC Section V Article 2 (Table T-274.2) and AWS D1.1 Clause 8 impose maximum permissible U g U_g U g thresholds based on material thickness:
Nominal Material Thickness Range Maximum Permissible Geometric Unsharpness ( U g U_g U g )
Under 2.0 in 2.0\text{ in} 2.0 in ( < 50 mm < 50\text{ mm} < 50 mm ) 0.020 in 0.020\text{ in} 0.020 in ( 0.51 mm 0.51\text{ mm} 0.51 mm )
2.0 to 3.0 in 2.0\text{ to }3.0\text{ in} 2.0 to 3.0 in ( 50 to 75 mm 50\text{ to }75\text{ mm} 50 to 75 mm ) 0.030 in 0.030\text{ in} 0.030 in ( 0.76 mm 0.76\text{ mm} 0.76 mm )
Over 3.0 to 4.0 in 3.0\text{ to }4.0\text{ in} 3.0 to 4.0 in ( 75 to 100 mm 75\text{ to }100\text{ mm} 75 to 100 mm ) 0.040 in 0.040\text{ in} 0.040 in ( 1.02 mm 1.02\text{ mm} 1.02 mm )
Greater than 4.0 in 4.0\text{ in} 4.0 in ( > 100 mm > 100\text{ mm} > 100 mm ) 0.070 in 0.070\text{ in} 0.070 in ( 1.78 mm 1.78\text{ mm} 1.78 mm )
- 3. Radiographic Sensitometry, Density & Film Viewing
- Optical Density Formulation
Radiographic film consists of a polyester base coated with a photographic emulsion of silver halide crystals ( A g B r AgBr A g B r ). Photons ionize halide atoms, creating a latent image reduced to metallic silver grains during chemical development. The blackening of the processed radiograph is quantified as Optical Density ( D D D ) : D = log 10 ( I 0 I t ) D = \log_{10}\left(\frac{I_0}{I_t}\right) D = lo g 10 ( I t I 0 )
where I 0 I_0 I 0 is the light intensity incident on the film from a calibrated industrial viewer, and I t I_t I t is the light intensity transmitted through the radiograph, measured via a calibrated transmission densitometer.
D = 1.0 ⟹ 10 % D = 1.0 \implies 10\% D = 1.0 ⟹ 10% of light transmitted ( 10 − 1 10^{-1} 1 0 − 1 ).
D = 2.0 ⟹ 1 % D = 2.0 \implies 1\% D = 2.0 ⟹ 1% of light transmitted ( 10 − 2 10^{-2} 1 0 − 2 ).
D = 3.0 ⟹ 0.1 % D = 3.0 \implies 0.1\% D = 3.0 ⟹ 0.1% of light transmitted ( 10 − 3 10^{-3} 1 0 − 3 ).
D = 4.0 ⟹ 0.01 % D = 4.0 \implies 0.01\% D = 4.0 ⟹ 0.01% of light transmitted ( 10 − 4 10^{-4} 1 0 − 4 ). HURTER & DRIFFIELD (H&D) CURVE
- Optical Density (D)
- ^
- 4.0 | .--- Shoulder (Saturation)
- | /
- 3.0 | / <-- Linear Region
- | / (Maximum Film Gradient & Contrast)
- 2.0 | /
- | .-----------' <-- Toe (Under-exposed, low contrast)
- 1.0 | /
- | _______________/
- +---+---+---+---+---+---+---+---+---+---> Log Relative Exposure
- Code Optical Density Boundaries (ASME Section V / AWS D1.1)
Single Film Viewing:
X-Ray Radiographs: Density must be within 1.8 ≤ D ≤ 4.0 1.8 \le D \le 4.0 1.8 ≤ D ≤ 4.0 throughout the area of interest.
Gamma-Ray Radiographs: Density must be within 2.0 ≤ D ≤ 4.0 2.0 \le D \le 4.0 2.0 ≤ D ≤ 4.0 throughout the area of interest.
Composite Viewing of Double Film Exposures: Density must be within 2.6 ≤ D ≤ 4.0 2.6 \le D \le 4.0 2.6 ≤ D ≤ 4.0 , with neither individual film falling below 1.3 1.3 1.3 .
Density Variation Limitations: The optical density across the weldment area of interest must not vary by more than − 15 % -15\% − 15% to + 30 % +30\% + 30% from the density measured through the body of the Image Quality Indicator (IQI).
4. Image Quality Indicators (IQI / Penetrameters) & Sensitivity Calibration
Radiographic sensitivity measures the smallest discontinuity that can be discerned on the film. Sensitivity is verified using Image Quality Indicators (IQIs) positioned on the weldment during exposure. HOLE-TYPE PLAQUE (ASTM E1025) WIRE-TYPE IQI (ASTM E747)
- T = 2% of Specimen Thickness 6 Graduated Wires
- +---------------------------+ +-----------------------+
- | (1T) (2T) (4T) | | | | | | | | |
- | o O ( ) | | | | | | | | |
- | Lead ID: "25" | | Lead ID: "SET B" |
- +---------------------------+ +-----------------------+
Hole Diameters: Essential Wire:
- 1T, 2T, 4T Plaque Thick. Must be Clearly Visible
- Plaque-Type vs. Wire-Type IQI Systems
Hole-Type Plaques (ASTM E1025): Rectangular metal strips manufactured from radiographically similar alloys. The plaque thickness ( T T T ) is typically fabricated to equal 2 % 2\% 2% of nominal weldment thickness . The plaque contains three drilled holes with diameters proportional to plaque thickness: 1 T 1T 1 T , 2 T 2T 2 T , and 4 T 4T 4 T .
Standard Radiographic Sensitivity (2-2T): The radiograph must clearly display the 2 % 2\% 2% thick plaque and resolve the 2 T 2T 2 T hole (whose diameter equals twice the plaque thickness, d = 2 T d = 2T d = 2 T ). Resolving the smaller 1 T 1T 1 T hole represents higher sensitivity ( 2 − 1 T 2-1T 2 − 1 T ).
Wire-Type IQIs (ASTM E747 / ISO 19232-1): Six plastic-encapsulated parallel wires of graduated diameters (Sets A, B, C, and D). ASTM E747 Table 4 establishes the mandatory Essential Wire Number that must be resolved across the weld area based on joint thickness.
Source-Side vs. Film-Side Placement Rules
Standard Source-Side Placement: Codes mandate placing the IQI on the source side of the joint (the side facing the radiation source), aligned parallel to and within 1 / 8 in 1/8\text{ in} 1/8 in ( 3.2 mm 3.2\text{ mm} 3.2 mm ) of the weld toe.
Film-Side Placement: When physical geometry precludes source-side access (e.g., closed pressure vessels, unpiggable pipelines), the IQI is placed on the film side. To warn the interpreter of lower sensitivity due to reduced penumbra magnification, a lead letter "F" at least 1 / 4 in 1/4\text{ in} 1/4 in ( 6.4 mm 6.4\text{ mm} 6.4 mm ) high must be placed immediately adjacent to the IQI on the film cassette.
Weld Reinforcement Shims: When a weld possesses high external crown reinforcement, the base metal under the IQI is thinner than the total weld cross-section. A radiographically similar compensating shim must be placed beneath the IQI to elevate it to the total thickness of the weld plus allowable reinforcement.