Study guide

15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice

AWS CWEng Certified Welding Engineer Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction & CWEng Exam Overview

About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set

2 Chapter 1: Mathematics & Statistics for Welding Engineers

1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers

3 Chapter 2: Physics Fundamentals & Mechanics

2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity

4 Chapter 3: General & Physical Chemistry for Welding

3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection

5 Chapter 4: Strength of Materials & Mechanics of Materials

4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment

6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding

5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments

7 Chapter 6: Electrical Engineering Principles for Welding Systems

6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow

8 Chapter 7: Welding Heat Sources & Arc Physics

7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design

9 Chapter 8: Arc Welding Processes & Parameter Controls

8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems

10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes

9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray

11 Chapter 10: Physical & Transformation Metallurgy of Steels

10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control

12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy

11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences

13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics

12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control

14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis

13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction

15 Chapter 14: Brazing, Soldering & Industrial Welding Safety

14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation

16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation

15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice

17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1

16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation

18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control

17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing

19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics

18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison

15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice

Key Takeaways Explain This Topic AI

Acceptance criteria are tighter for cyclically loaded connections than for statically loaded ones, so the same indication can pass in one structure and fail in another.

Holding time for post-weld heat treatment is set per unit of thickness with a stated minimum, and both the rate limits and the soak must be recorded.

Heating and cooling rate limits exist to prevent thermal gradients from generating new residual stress during the very cycle intended to relieve it.

Visual inspection is a code-mandated examination in its own right, not a preliminary to volumetric testing.

Last updated: September 2026

Non-Destructive Examination (NDE) Code Protocols (Clause 8 Part C)

Visual testing is complemented by surface and volumetric NDE specified in contract documents:

Magnetic Particle Testing (MT): Governed by ASTM E709. Mandated on cut edges after discontinuity removal and on heavy weld passes to detect surface/subsurface cracks.

Ultrasonic Testing (UT): Governed by AWS D1.1 Clause 8 Part F. Utilizes straight-beam and angle-beam transducers (45°, 60°, 70°) calibrated against an IIW reference block. Indications are evaluated based on decibel attenuation ratings:

d = a - b - c

where a is the test indication level (dB), b is the reference level (dB), and c is the sound path attenuation factor (c = (path - 1 in) x 2). Severity levels determine acceptance (Class A through D per Table 8.2 and Table 8.3).

Delayed Inspection Rule (Clause 8.15): For high-strength steels with Fy >= 70 ksi (Group IV or Q&T steels), final VT and NDE must be delayed for at least 48 hours after weld completion to allow any latent hydrogen-induced cold cracking to initiate and propagate to detectable size.

  • Comprehensive Worked Engineering Example: PWHT Schedule Calculation & CWI Visual Audit
  • Problem Statement

A heavy bridge crane runway box girder fabricated from ASTM A572 Grade 50 steel has a maximum flange thickness of t = 3.5 in (88.9 mm) and is welded to a 1.25 in (31.8 mm) web plate using FCAW-G. The project specification mandates a furnace Post-Weld Heat Treatment per AWS D1.1 Clause 7.8, followed by a Certified Welding Inspector (CWI) visual audit per Table 8.1 (Cyclically Loaded).

Part A: PWHT Schedule Calculation Calculate:

The minimum required soak holding time at 1150°F (620°C).

The maximum allowable heating rate above 600°F (315°C).

The maximum allowable cooling rate above 600°F (315°C).

The total minimum time elapsed during the controlled thermal cycle above 600°F.

Part B: CWI Visual Audit Evaluation During the post-PWHT visual audit, the inspector records three specific observations:

Observation 1: On the tension flange transverse CJP butt splice, the toe undercut depth is measured at 0.018 in (0.46 mm).

Observation 2: On a longitudinal web-to-flange fillet weld, two surface pores of diameter 1/16 in (1.6 mm) are found spaced 6 inches (150 mm) apart.

Observation 3: A continuous 12 mm specified fillet weld has a measured leg size of 10.5 mm (1.5 mm ~ 1/16 in undersize) along a 150 mm stretch of an 1800 mm continuous joint, located in the middle third of the girder span.

Determine whether each observation is Acceptable or Rejectable under Table 8.1 cyclically loaded criteria. PWHT TEMPERATURE PROFILE CALCULATION

  • 1150°F + - - - - - - - - - - +-----------------------+ - - - - - - - - - - - -
  • | / Soak Time = 2.375 hr | Cooling Rate
  • | Heating Rate / (2 hr 23 min) | R_C = 142.9°F/hr
  • | R_H = 114.3°F / | (t_cool = 3.85 hr)
  • | (t_heat = 4.81h)/ |
  • 600°F +----------------+ +-------------------
  • |<-------------- Total Cycle Above 600°F = 11.035 hr -------------->|
  • Step-by-Step Engineering Solution
  • Part A: PWHT Schedule Calculations
  • Step 1: Soak Holding Time

Thickness of thickest section joined: t = 3.5 in (88.9 mm).

Per AWS D1.1 Clause 7.8.1, for thickness exceeding 2.0 in:

  • t_soak = 2.0 hr + 0.25 hr x (t - 2.0 in)
  • t_soak = 2.0 hr + 0.25 hr x (3.5 - 2.0) = 2.0 + 0.375 = 2.375 hr
  • t_soak = 2 hours and 22.5 minutes (~ 2 hr 23 min)
  • Step 2: Maximum Heating Rate Above 600°F

Per Clause 7.8.1:

R_H = (400°F/hr) / t = 400 / 3.5 = 114.29°F/hr

Code bounds check: 100°F/hr <= R_H <= 400°F/hr. Since 114.29°F/hr > 100°F/hr, the maximum heating rate is 114.3°F/hr (63.5°C/hr).

Step 3: Maximum Cooling Rate Above 600°F

Per Clause 7.8.1:

R_C = (500°F/hr) / t = 500 / 3.5 = 142.86°F/hr

Code bounds check: 100°F/hr <= R_C <= 500°F/hr. The maximum allowable cooling rate is 142.9°F/hr (79.4°C/hr).

Step 4: Total Minimum Thermal Cycle Duration Above 600°F

Heating temperature rise from 600°F to 1150°F:

Delta T = 1150°F - 600°F = 550°F

Minimum heating time:

t_heat = 550°F / (114.29°F/hr) = 4.8125 hr (4 hr 49 min)

Minimum cooling time:

t_cool = 550°F / (142.86°F/hr) = 3.8500 hr (3 hr 51 min)

Total cycle time above 600°F:

  • t_total = t_heat + t_soak + t_cool = 4.8125 + 2.3750 + 3.8500 = 11.0375 hr
  • Total Duration Above 600°F = 11 hours and 2.25 minutes (~ 11 hr 2 min)
  • Part B: CWI Visual Audit Disposition

Observation 1 (Transverse CJP Butt Undercut = 0.018 in):

Joint is in a crane runway girder subjected to cyclic fatigue, and the butt weld is transverse to tension.

Per Table 8.1 (Cyclically Loaded Nontubular), undercut transverse to tensile stress must not exceed 0.01 in (0.25 mm) .

Measured undercut is 0.018 in > 0.01 in.

Disposition: REJECTABLE. The undercut notch must be excavated by light grinding or filled with a qualified TIG/SMAW repair pass and ground smooth.

Observation 2 (Fillet Porosity: two 1/16 in pores spaced 6 in apart):

Joint is a longitudinal fillet weld in a cyclically loaded member.

Per Table 8.1, maximum allowable diameter is 3/32 in (2.4 mm), and frequency must not exceed one pore in 4 inches (100 mm).

Pore diameter (1/16 in = 0.0625 in) is less than 3/32 in (0.0938 in). Pore spacing (6 in) exceeds the 4 in minimum separation.

Disposition: ACCEPTABLE.

Observation 3 (Fillet Undersize: 1.5 mm on 150 mm of 1800 mm weld):

Measured undersize: 12 mm - 10.5 mm = 1.5 mm (< 1/16 in / 1.6 mm). Complies with undersize threshold.

Length percentage: 150 mm / 1800 mm = 8.33% <= 10%. Complies with cumulative length limit.

Location check: The defect is in the middle third of the girder span, not at girder ends (no restriction regarding the 2 x bf end zone applies).

Disposition: ACCEPTABLE.

  • Industrial Scenarios & Certified Welding Engineer Exam Pitfalls
  • Real-World Field Disaster Scenario

A heavy open-pit mining dragline boom fabricated from quenched and tempered ASTM A514 Grade B steel (Fy = 100 ksi) underwent major field splice modifications. The repair contractor's quality manager, accustomed to conventional carbon steel piping codes (ASME B31.3), instituted a Post-Weld Heat Treatment at 1250°F (675°C) for two hours to "relieve residual stresses." During the subsequent shift under full digging payload, the entire upper boom structure buckled catastrophically. The metallurgical failure investigation revealed that because the 1250°F PWHT temperature far exceeded the mill tempering temperature (1150°F), the quenched martensite had completely over-tempered, coalescing carbides and dropping the yield strength from 100 ksi to 54 ksi (46% loss of capacity). The contractor was held liable for $12 million in equipment replacement and lost mine production.

Certified Welding Engineer Exam Pitfalls

Exam Trap 1: The Soak Time Over 2 Inches Formula When calculating PWHT soak times for plates thicker than 2 in, candidates often mistakenly apply 1 hr/inch across the entire thickness (e.g., calculating 4 hours for a 4 in plate). Per AWS D1.1 Clause 7.8.1, the rule changes after 2 inches: it is 2 hours for the first 2 inches, plus only 15 minutes for each additional inch ! For a 4 in plate: t = 2.0 + (2 x 0.25) = 2.5 hours. Calculating 4 hours is a classic exam failure.

Exam Trap 2: The Undercut Threshold Trap Exam questions routinely test whether candidates know the difference between static and cyclic undercut limits. For a static building frame, an undercut of 0.03 in (1/32 in) is completely acceptable. For a cyclically loaded bridge or crane girder tension member, that exact same 0.03 in undercut is a severe violation, because the code enforces an absolute cap of 0.01 in (0.25 mm) .

Exam Trap 3: Cooling Below 600°F An exam question will ask for the required furnace cooling rate between 600°F and room temperature. The answer is: None. Below 600°F (315°C), the furnace may be opened, and the assembly cooled in still air.