Study guide

15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria

AWS CWEng Certified Welding Engineer Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction & CWEng Exam Overview

About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set

2 Chapter 1: Mathematics & Statistics for Welding Engineers

1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers

3 Chapter 2: Physics Fundamentals & Mechanics

2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity

4 Chapter 3: General & Physical Chemistry for Welding

3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection

5 Chapter 4: Strength of Materials & Mechanics of Materials

4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment

6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding

5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments

7 Chapter 6: Electrical Engineering Principles for Welding Systems

6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow

8 Chapter 7: Welding Heat Sources & Arc Physics

7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design

9 Chapter 8: Arc Welding Processes & Parameter Controls

8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems

10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes

9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray

11 Chapter 10: Physical & Transformation Metallurgy of Steels

10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control

12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy

11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences

13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics

12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control

14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis

13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction

15 Chapter 14: Brazing, Soldering & Industrial Welding Safety

14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation

16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation

15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice

17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1

16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation

18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control

17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing

19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics

18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison

15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria

Key Takeaways Explain This Topic AI

AWS D1.1 Clause 7.8 governs Post-Weld Heat Treatment (PWHT) for carbon steels, specifying a holding range of 1100°F - 1200°F (590°C - 650°C) to relax residual stresses through high-temperature creep and temper hard HAZ microstructures.

Above 600°F (315°C), heating rates are capped at 400°F/hr divided by thickness in inches (maximum 400°F/hr, minimum 100°F/hr) and cooling rates at 500°F/hr divided by thickness, with soak times of 1 hr/in up to 2 in plus 15 min per additional inch.

PWHT is generally prohibited or restricted for Quenched and Tempered (Q&T) steels like ASTM A514/A517, where holding temperatures must never exceed 1150°F (620°C) to avoid destroying the tempered martensite microstructure and degrading tensile strength.

Visual inspection per Table 8.1 strictly prohibits cracks and lack of fusion across all structures, but establishes vital operational distinctions: cyclically loaded tension welds cap undercut at 0.01 in (0.25 mm) compared to 1/32 in (1 mm) for static structures.

Piping porosity in CJP butt welds transverse to tensile stress is prohibited in both static and cyclic categories; in other welds, cyclic loading permits only one pore per 4 inches (d <= 3/32 in), whereas static loading permits up to 3/8 in accumulated porosity per linear inch.

Last updated: September 2026

15.3 Post-Weld Heat Treatment (PWHT) & Visual/NDE Acceptance Criteria

Quick Answer: AWS D1.1 Clause 7.8 governs Post-Weld Heat Treatment (PWHT) for carbon steels, specifying a holding range of 1100°F - 1200°F (590°C - 650°C) to relax residual stresses through high-temperature creep and temper hard HAZ microstructures. Above 600°F (315°C), heating rates are capped at 400°F/hr divided by thickness in inches (maximum 400°F/hr, minimum 100°F/hr) and cooling rates at 500°F/hr divided by thickness, with soak times of 1 hr/in up to 2 in plus 15 min per additional inch. Visual inspection per Table 8.1 strictly prohibits cracks and lack of fusion across all structures, but establishes vital operational distinctions: cyclically loaded tension welds cap undercut at 0.01 in (0.25 mm) compared to 1/32 in (1 mm) for static structures, while cyclic porosity is restricted to one pore per 4 inches of weld (d <= 3/32 in).

Post-Weld Heat Treatment (PWHT) Engineering Fundamentals (Clause 7.8)

During arc welding, steep thermal gradients and localized weld metal solidification induce severe tensile residual stresses that reach or exceed the room-temperature yield strength (Fy) of the base metal. In heavy structural weldments subjected to dynamic fatigue, stress corrosion cracking (SCC), or low-temperature impact service, Post-Weld Heat Treatment (PWHT) —also designated thermal stress relief—is mandated by design specifications to restore mechanical integrity.

Metallurgical Mechanisms of Thermal Stress Relief

Thermal stress relief does not alter the fundamental macro-geometry of the weldment; rather, it operates via two distinct metallurgical phenomena:

Yield Strength Reduction & Creep Relaxation: As structural steel is heated into the subcritical range (590°C - 650°C / 1100°F - 1200°F), its yield strength plummets to roughly 10% to 20% of its ambient room-temperature value. Residual elastic strain (e_e) converts into plastic strain (e_p) and time-dependent creep strain (e_c):

e_total = e_e + e_p + e_c

Because the material can no longer support high elastic stresses at elevated temperatures, peak residual stresses relax down to the elevated-temperature yield strength (< 5-8 ksi / 35-55 MPa).

HAZ Tempering & Hydrogen Effusion: Holding at 1100°F - 1200°F tempers hard, brittle martensite and bainite in the Coarse-Grained Heat-Affected Zone (CGHAZ). High-carbon martensitic laths decompose into soft, ductile ferrite and coarsened cementite (carbide spherodization), reducing peak HAZ hardness below 22 HRC (250 HV). Simultaneously, high thermal kinetic energy accelerates the effusion of any residual diffusible hydrogen from the crystal lattice. RESIDUAL STRESS RELAXATION DURING PWHT CYCLE

  • Stress Level (ksi)
  • ^
  • 50 +---------------------------+ <-- Ambient Room-Temp Yield (~50 ksi)
  • | Peak As-Welded |
  • 40 | Residual Stress v

| .

30 | .

| .

20 | .

  • | +-------------------------+
  • 10 | | Stress Relaxed to |
  • | | Elevated-Temp Yield |
  • 0 +---------------------------------+-------------------------> Temperature
  • Ambient (70°F) 600°F 1150°F (PWHT)
  • The Quenched and Tempered (Q&T) Steel Danger (ASTM A514 / A517)

Critical Caution: PWHT on High-Strength Q&T Steels High-strength quenched and tempered steels (e.g., ASTM A514, with Fy = 100 ksi) derive their strength from a carefully tempered martensitic microstructure achieved at mill tempering temperatures of 1150°F - 1250°F. Subjecting A514 weldments to indiscriminate PWHT can be catastrophic. If the PWHT holding temperature exceeds the original tempering temperature, the steel over-tempers, causing an irreversible 30% to 50% drop in tensile and yield strength . Furthermore, PWHT of high-alloy Q&T steels induces reheat cracking (stress-relief cracking) along CGHAZ prior-austenite grain boundaries. AWS D1.1 Clause 7.8 strictly mandates that PWHT of A514/A517 steels shall not exceed 1150°F (620°C) and requires engineering concurrence.

AWS D1.1 Thermal Cycle Specifications & Governing Equations

AWS D1.1 Clause 7.8 establishes rigorous limits on holding temperatures, heating rates, soak durations, cooling rates, and furnace temperature uniformity to prevent thermal shock and severe thermal gradient-induced distortion. AWS D1.1 PWHT THERMAL CYCLE PROFILE

  • Temperature (°F)
  • ^
  • | Soak Period (t_soak)
  • 1150°F | +-------------------------+
  • | / 1100°F - 1200°F Holding |
  • | Controlled / (1 hr/in <=2", +15m) | Controlled Cooling
  • | Heating Rate / | (R_C <= 500/t)
  • 600°F + - - - - - - - - + - - - - - - - - - - - - - - - + - - - - - - - -
  • | Unrestricted / | Air Cool
  • | Heating (<600) | (<600°F)
  • 70°F +---------------+---------------------------------+-------------> Time
  • 1. Holding Temperature Ranges

Carbon Steels (Groups I, II, III): 1100°F to 1200°F (590°C to 650°C).

Low-Alloy Steels (Group IV): 1100°F to 1250°F (590°C to 675°C).

2. Heating Rate Restrictions (T > 600°F / 315°C)

Below 600°F, heating rate is unrestricted. Above 600°F, the rate of heating (R_H) must not exceed:

R_H = (400°F/hr) / t (in) = (222°C/hr) / (t / 25.4 mm)

Maximum Ceiling: In no case shall R_H exceed 400°F/hr (222°C/hr).

Minimum Floor: R_H need not be less than 100°F/hr (56°C/hr), regardless of thickness.

3. Holding Time (Soak Duration)

The holding time at temperature (t_soak) is dictated by the thickest section joined:

Thickness t <= 2.0 in (50 mm): 1 hour per inch (2.36 min/mm) of thickness, with a minimum holding time of 15 minutes for sections under 1/4 in.

Thickness t > 2.0 in (50 mm): 2 hours plus 15 minutes for each additional inch (0.59 min/mm) of thickness over 2.0 in:

  • t_soak = 2.0 hr + 0.25 hr x (t - 2.0 in)
  • 4. Cooling Rate Restrictions (T > 600°F / 315°C)

Above 600°F, cooling must proceed in a closed furnace or chamber at a rate (R_C) not exceeding:

R_C = (500°F/hr) / t (in) = (278°C/hr) / (t / 25.4 mm)

Maximum Ceiling: In no case shall R_C exceed 500°F/hr (278°C/hr).

Minimum Floor: R_C need not be less than 100°F/hr (56°C/hr).

Below 600°F (315°C): The weldment may be removed from the furnace and cooled in still air.

5. Temperature Uniformity in Furnace

During heating and cooling, the variation in temperature throughout the component must not exceed 250°F (140°C) within any 15 ft (4.6 m) interval. During the holding soak period, the temperature across the entire component must remain within a 50°F (28°C) band.

Visual Inspection Acceptance Criteria: AWS D1.1 Table 8.1

Visual Testing (VT) is the foundational Quality Assurance method in AWS D1.1 Clause 8. Every weld must be visually inspected along its entire length. AWS D1.1 Table 8.1 ( Visual Inspection Acceptance Criteria ) establishes fundamentally different criteria depending on whether a structure is statically loaded (buildings) or cyclically loaded (bridges, crane girders). +---------------------------------------------------------------------------------------------------------+

  • | AWS D1.1 TABLE 8.1 VISUAL INSPECTION ACCEPTANCE CRITERIA MATRIX |
  • +----------------------------+------------------------------------+---------------------------------------+
  • | Discontinuity Category | Statically Loaded Nontubular | Cyclically Loaded Nontubular |
  • +----------------------------+------------------------------------+---------------------------------------+
  • | 1. Crack Prohibition | NO CRACKS PERMITTED | NO CRACKS PERMITTED |
  • | | (Zero tolerance, any size) | (Zero tolerance, any size) |
  • +----------------------------+------------------------------------+---------------------------------------+
  • | 2. Weld/Base Metal Fusion | Complete fusion required between | Complete fusion required between |
  • | | passes and weld to base metal | passes and weld to base metal |
  • +----------------------------+------------------------------------+---------------------------------------+
  • | 3. Crater Cross-Section | All craters filled to full weld | All craters filled to full weld |
  • | | cross-section (except ends) | cross-section (except ends) |
  • +----------------------------+------------------------------------+---------------------------------------+
  • | 4. Fillet Weld Undersize | Leg undersize <= 1/16" (1.6 mm) on | Leg undersize <= 1/16" (1.6 mm) on |
  • | | max 10% of length; ends restricted | max 10% of length; ends restricted |
  • +----------------------------+------------------------------------+---------------------------------------+
  • | 5. Maximum Undercut | <= 1/32" (1 mm) general; | Transverse to tension: <= 0.01" |
  • | | <= 1/16" (1.6 mm) on accum 2" in 12" | (0.25 mm) STRICT MAXIMUM; |
  • | | | All other cases: <= 1/32" (1 mm) |
  • +----------------------------+------------------------------------+---------------------------------------+
  • | 6. Porosity Limits | CJP Butt: NO piping porosity | CJP Butt: NO piping porosity |
  • | | Other: Sum of dia >= 1/32" shall | Other: Frequency <= 1 pore in 4" |
  • | | not exceed 3/8" in 1" & 3/4" in 12" | (100 mm); Max dia <= 3/32" (2.5 mm) |

+----------------------------+------------------------------------+---------------------------------------+ CRITICAL UNDERCUT THRESHOLDS: STATIC VS CYCLIC

  • STATIC CONNECTIONS CYCLIC TENSION CONNECTIONS
  • ================== ==========================
  • Max Undercut = 1/32" (1.0 mm) Max Undercut = 0.01" (0.25 mm)
  • +---------------------------+ +---------------------------+
  • | Weld Crown | | Weld Crown |
  • ---+ +---- ----+ +----
  • | | | |
  • v v v v
  • h <= 1/32" (1.0 mm) h <= 0.01" (0.25 mm)
  • (Permits up to 1/16" on accum 2" in 12") (STRICT ZERO-TOLERANCE TO DEEP NOTCHES)
  • In-Depth Analysis of Table 8.1 Discontinuity Rules
  • 1. Crack Prohibition

Under no circumstances does AWS D1.1 permit cracks, microcracks, or crater cracks. Any crack detected visually, via Liquid Penetrant (PT), Magnetic Particle (MT), or Ultrasonic Testing (UT) constitutes immediate rejection and requires complete excavation and repair.

2. Undercut Limits: The 0.01 in Cyclic Rule

In statically loaded structures, undercut is permitted up to 1/32 in (1.0 mm) along the entire length, and up to 1/16 in (1.6 mm) for an accumulated length of 2 inches (50 mm) in any 12 inches (300 mm) of weld.

In cyclically loaded structures subjected to calculated tensile stress normal to the weld axis, undercut must not exceed 0.01 in (0.25 mm) . This microscopic threshold (250 micro-m) exists because toe undercut in cyclic tension creates an acute stress concentration notch that drastically slashes fatigue initiation life.

3. Fillet Weld Undersize Allowance

Table 8.1 permits a fillet weld leg size to be undersized by up to 1/16 in (1.6 mm) without correction, provided that:

The undersized portion does not exceed 10% of the continuous weld length .

On girder web-to-flange welds, no undersize is permitted at the ends for a distance equal to twice the flange width (2 x bf), where end shears and principal stress rotations peak.

4. Convexity and Weld Reinforcement Limits

For fillet welds, face convexity (C) must not exceed the limits shown below, based on weld face width (W):

  • W <= 5/16 in (8 mm): C_max = 1/16 in (1.6 mm)
  • 5/16 in < W < 1 in (25 mm): C_max = 1/8 in (3.2 mm)
  • W >= 1 in (25 mm): C_max = 3/16 in (4.8 mm)

Formula: C <= 0.1 W + 0.03 in (1 mm).

Groove weld face reinforcement must not exceed 1/8 in (3.2 mm) and must blend smoothly with the parent plate without sharp weld toe re-entrant corners.

5. Porosity Limitations

Complete Joint Penetration (CJP) Butt Welds Transverse to Tension: In both static and cyclic structures, zero visible piping porosity is permitted. Volumetric sound weld metal is non-negotiable.

Other Groove & Fillet Welds (Static): The sum of visible piping porosity 1/32 in (1 mm) or larger in diameter must not exceed 3/8 in (10 mm) in any linear inch of weld, and must not exceed 3/4 in (20 mm) in any 12 in (300 mm) length.