Study guide
17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations
Key Takeaways Explain This Topic AI
5xxx series aluminum alloys containing more than 3.0% magnesium (including ER5356 and 5083) are metallurgically prohibited from continuous service above 65°C (150°F) due to continuous grain boundary beta-phase (Mg2Al3) sensitization and stress corrosion cracking.
ER4043 resists solidification cracking through its silicon content but cannot be strengthened by post-weld heat treatment and anodises dark.
ER5356 gives higher strength and better colour match after anodising but must not be used where sustained service above roughly 65 degrees C could cause stress-corrosion-susceptible phase precipitation in high-magnesium deposits.
Dissimilar carbon-to-stainless joints are commonly made with a 309-type filler because its high chromium and nickel equivalents tolerate dilution from the carbon steel side.
Dilution must be estimated before the deposit chemistry is predicted, since the filler classification alone does not describe the metal that ends up in the joint.
Last updated: September 2026
Aluminum Filler Metal Selection: AWS A5.10
Welding aluminum alloys requires careful consumable matching per AWS A5.10 / A5.10M ( Bare Aluminum and Aluminum-Alloy Welding Electrodes and Rods ). The primary engineering decision in structural aluminum fabrication is choosing between the two workhorse consumables: ER4043 and ER5356 . +-----------------------------------------------------------------------------------------+
- | ER4043 VS. ER5356 COMPARISON MATRIX |
- +------------------------------------+--------------------------+-------------------------+
- | Characteristic | AWS A5.10 ER4043 | AWS A5.10 ER5356 |
- +------------------------------------+--------------------------+-------------------------+
- | Principal Alloying System | Al - 5.0% Si | Al - 5.0% Mg |
- | Solidification Cracking Resistance | Superior (Al-Si eutectic)| Lower (requires strict |
- | | heals freezing fissures) | dilution management) |
- | Weld Pool Fluidity & Wetting | Exceptional (flows easily| Viscous, fast-freezing, |
- | | with bright appearance) | requires weaving |
- | All-Weld Shear Strength | Low (~11–13 ksi / 80 MPa)| High (~17–20 ksi / 130 |
- | | | MPa; 30-50% stronger!) |
- | Ductility & Impact Toughness | Moderate | High |
- | Post-Weld Anodizing Color Match | Poor: turns dark gray / | Excellent: bright silver|
- | (on 6061 base metal) | charcoal-black | matches base metal |
- | Continuous Service Temperature | Unrestricted | STRICTLY RESTRICTED TO |
- | | (up to ~150°C / 300°F) | T < 65°C (150°F)! |
- +------------------------------------+--------------------------+-------------------------+
- The 65°C (150°F) Service Temperature Limit for 5xxx Alloys
CWEng Critical Metallurgy Rule: The Sensitization of 5xxx Alloys Any 5xxx series aluminum alloy or weld deposit containing more than 3.0% Magnesium (such as ER5356 with ~5.0% Mg, ER5183 with ~4.8% Mg, and base metal 5083 with ~4.5% Mg) is metallurgically unstable at sustained temperatures above 65°C (150°F) . SENSITIZATION MECHANISM IN AL-MG ALLOYS (> 65°C)
- Solid Solution Alpha Matrix (Al) Grain Boundary
- +------------------------------------+--------------------------------+
- | High Magnesium in Solution (~5% Mg)| |
- | | Continuous Network of |
- | [Mg] ----------> | Beta-Phase (Mg2Al3) Film |
- | | - Highly Anodic (-1.24 V) |
- | | - Rapidly Corrodes |
- +------------------------------------+--------------------------------+
At temperatures exceeding 65°C, excess magnesium precipitates out of the alpha-aluminum solid solution, forming continuous grain boundary films of the intermetallic compound beta-phase (Mg2Al3) .
In the galvanic series, beta-phase is extremely anodic (-1.24 V vs SCE) compared to the surrounding alpha-aluminum matrix (-0.84 V vs SCE).
In the presence of an electrolyte (marine spray, road deicing salts, or industrial condensate) and sustained tensile stress, galvanic dissolution of the beta-phase network causes rapid Stress Corrosion Cracking (SCC) and catastrophic intergranular exfoliation.
Mandatory Rule: For aluminum structural applications exposed to temperatures >= 65°C (150°F)—such as truck bulkheads, engine brackets, and chemical heat exchangers—the engineer must specify ER4043 or low-magnesium ER5554 (Al - 2.7% Mg).
- Comprehensive Worked Engineering Example: Dissimilar Metal Weld Dilution & FN Prediction
- Problem Statement
A chemical reactor vessel involves a circumferential butt weld joining ASTM A36 carbon steel to AISI 304L austenitic stainless steel . The joint is welded via mechanized GMAW with an AWS A5.9 ER309L solid wire.
From procedure qualification macroetch measurements, the total joint dilution is D_total = 0.26 (26%), consisting of equal 13% dilution from each base metal (D_A36 = 0.13, D_304L = 0.13). The filler metal provides the remaining fraction: f_wire = 1.00 - 0.26 = 0.74.
The measured certified material test report (CMTR) compositions are:
ASTM A36: 0.18% C, 0.80% Mn, 0.25% Si, 0.05% Cr, 0.05% Ni, 0.008% N, 0.02% Mo, 0.15% Cu, 0.00% Nb.
AISI 304L: 0.022% C, 1.45% Mn, 0.45% Si, 18.30% Cr, 8.20% Ni, 0.065% N, 0.20% Mo, 0.20% Cu, 0.00% Nb.
ER309L: 0.018% C, 1.70% Mn, 0.40% Si, 23.50% Cr, 13.40% Ni, 0.045% N, 0.15% Mo, 0.10% Cu, 0.00% Nb.
Calculate:
The Chromium Equivalent (Cr_eq) and Nickel Equivalent (Ni_eq) for each base metal and the filler metal using WRC-1992 formulas.
The final diluted weld metal Cr_eq and Ni_eq.
The predicted Ferrite Number (FN) and verify that the weld avoids both solidification cracking and martensite. DILUTION LEVER RULE TRIANGLE
- ER309L Filler Metal (74%)
- /\
- / \
- / \
- / * \ <-- Weld Metal Puddle Position
- / \
- /__________\
- ASTM A36 (13%) AISI 304L (13%)
- Step-by-Step Solution
Step 1: Compute WRC-1992 Equivalents for Constituents C r e q = % C r + % M o + 0.7 % N b Cr_{eq} = \%Cr + \%Mo + 0.7 \%Nb C r e q = % C r + % M o + 0.7% N b N i e q = % N i + 35 % C + 20 % N + 0.25 % C u Ni_{eq} = \%Ni + 35 \%C + 20 \%N + 0.25 \%Cu N i e q = % N i + 35% C + 20% N + 0.25% C u
- For ASTM A36 Base Metal: Cr_eq(A36) = 0.05 + 0.02 + 0 = 0.07%
- Ni_eq(A36) = 0.05 + 35(0.18) + 20(0.008) + 0.25(0.15) = 0.05 + 6.30 + 0.16 + 0.0375 = 6.55%
- For AISI 304L Base Metal: Cr_eq(304L) = 18.30 + 0.20 + 0 = 18.50%
- Ni_eq(304L) = 8.20 + 35(0.022) + 20(0.065) + 0.25(0.20) = 8.20 + 0.77 + 1.30 + 0.05 = 10.32%
- For ER309L Filler Metal: Cr_eq(wire) = 23.50 + 0.15 + 0 = 23.65%
- Ni_eq(wire) = 13.40 + 35(0.018) + 20(0.045) + 0.25(0.10) = 13.40 + 0.63 + 0.90 + 0.025 = 14.96%
Step 2: Calculate Diluted Weld Metal Equivalents C r e q ( weld ) = 0.13 ( C r e q ( A36 ) ) + 0.13 ( C r e q ( 304L ) ) + 0.74 ( C r e q ( wire ) ) Cr_{eq(\text{weld})} = 0.13(Cr_{eq(\text{A36})}) + 0.13(Cr_{eq(\text{304L})}) + 0.74(Cr_{eq(\text{wire})}) C r e q ( weld ) = 0.13 ( C r e q ( A36 ) ) + 0.13 ( C r e q ( 304L ) ) + 0.74 ( C r e q ( wire ) )
Cr_eq(weld) = 0.13(0.07) + 0.13(18.50) + 0.74(23.65) = 0.0091 + 2.405 + 17.501 = 19.92% N i e q ( weld ) = 0.13 ( N i e q ( A36 ) ) + 0.13 ( N i e q ( 304L ) ) + 0.74 ( N i e q ( wire ) ) Ni_{eq(\text{weld})} = 0.13(Ni_{eq(\text{A36})}) + 0.13(Ni_{eq(\text{304L})}) + 0.74(Ni_{eq(\text{wire})}) N i e q ( weld ) = 0.13 ( N i e q ( A36 ) ) + 0.13 ( N i e q ( 304L ) ) + 0.74 ( N i e q ( wire ) )
- Ni_eq(weld) = 0.13(6.55) + 0.13(10.32) + 0.74(14.96) = 0.8515 + 1.3416 + 11.0704 = 13.26%
- Step 3: Ferrite Number (FN) Prediction & Microstructural Verification
Ratio calculation: Cr_eq / Ni_eq = 19.92 / 13.26 = 1.502.
On the WRC-1992 diagram, the solidification mode boundary between AF and FA occurs at Cr_eq / Ni_eq ≈ 1.48. Since 1.502 > 1.48, the weld solidifies via the primary ferrite (FA) mode .
Evaluating the WRC-1992 iso-ferrite line in this coordinate region yields 6.2 FN .
Conclusion: The calculated Ferrite Number of 6.2 FN sits safely inside the ideal 3 to 10 FN design window. The weld completely avoids the martensite boundary (which requires Cr_eq < 17% at Ni_eq = 13.26%) and possesses robust resistance to solidification hot cracking.
- Industrial Scenarios & Certified Welding Engineer Exam Traps
- Real-World Field Disaster Scenario
A chemical processing facility built an insulated storage tank for hot nitric acid wash solution operating at 80°C (176°F). The structural design specified 5083-H116 aluminum plates joined with ER5356 filler metal to take advantage of 5356's high transverse fillet shear strength. After 14 months of leak-free operation, the entire lower shell-to-bottom fillet joint ruptured catastrophically around 75% of the circumference. Metallographic failure analysis revealed extensive intergranular stress corrosion cracking (SCC) filled with aluminum hydroxide corrosion product. The welding engineer failed to recognize that operating ER5356 (5% Mg) above 65°C caused continuous beta-phase (Mg2Al3) precipitation at grain boundaries, which rapidly dissolved under operating tensile stress in the slightly acidic environment. The entire vessel had to be scrapped and rebuilt using ER4043.
Certified Welding Engineer Exam Traps
Exam Trap 1: ER309L at High Temperatures (> 425°C) Exam questions routinely describe a dissimilar joint between ASTM A387 Gr 11 (Cr-Mo) and 316H stainless in an oil refinery furnace operating at 540°C (1000°F), asking candidates to select the proper filler metal. Candidates instinctively select ER309L. This is wrong! At 540°C, ER309L causes severe carbon migration, forming a brittle decarburized groove in the A387 steel. The correct answer is a nickel-base filler metal: ERNiCr-3 (Inconel 82) or ERNiCrMo-3 (Inconel 625) .
Exam Trap 2: Post-Weld Anodizing of 6061 Welded with ER4043 An architect specifies 6061-T6 aluminum handrails with a decorative clear-anodized finish. The shop welds the joints using ER4043 due to its excellent weldability. Upon anodizing, every single weld seam turns an unsightly charcoal-black color, resulting in total rejection. The exam tests your knowledge that ER4043 contains 5% silicon which forms black elemental silicon particles upon anodizing , whereas ER5356 produces an excellent silvery color match .
Exam Trap 3: Ferrite Measurement Units: Percent vs. Ferrite Number Questions test whether candidates know that ferrite in stainless steel is legally measured in Ferrite Number (FN) per AWS A4.2 and ISO 8249, not percent ferrite (% ferrite) . While FN roughly approximates volume percentage below 10 FN, magnetic measurement instruments calibrate strictly against NIST primary standards in FN. Expressing ferrite as '%' on a certified welding document is technically non-compliant.