Study guide
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications
Key Takeaways Explain This Topic AI
AWS A5 specification architecture categorizes filler metals and fluxes by welding process, base alloy system, and mandatory mechanical and chemical testing schedules governed by AWS A5.01.
SMAW classifications under AWS A5.1 and A5.5 define minimum tensile strength, all-position or flat/horizontal capability, coating chemistry, and operating current/polarity, with low-alloy suffix designators (-A1, -B2, -C3, -D2, -M) specifying exact weld metal metallurgy.
Solid GMAW/GTAW wires under AWS A5.18 and A5.28 rely on precise deoxidation balances (Si, Mn, Ti, Zr, Al), where ER70S-2 provides triple-deoxidized tolerance for rusty/scaled steel and ER70S-6 provides high Si-Mn fluidity for superior wetting and CVN toughness.
FCAW consumables under AWS A5.20 and A5.29 differentiate between gas-shielded rutile/basic systems (E70T-1, E71T-1) and self-shielded systems (E71T-8), the latter utilizing Al-Mg deoxidizers critical for demand-critical seismic connections under AWS D1.8.
Last updated: September 2026
17.1 AWS A5 Consumables: Carbon & Low-Alloy Steels
Quick Answer: The American Welding Society (AWS) A5 series provides the regulatory and metallurgical framework for welding consumables. Carbon steel SMAW electrodes are governed by AWS A5.1 (e.g., E7018 basic low-hydrogen, E6010 cellulosic deep-penetration, E7024 high-deposition rutile/iron powder), while low-alloy electrodes fall under AWS A5.5 with compositional suffixes (-A1 C-Mo, -B2 Cr-Mo, -C3 Ni-alloy, -D2 Mn-Mo, -M military high-toughness). Solid GMAW wires follow AWS A5.18 (ER70S-2 triple-deoxidized, ER70S-6 high Si-Mn) and AWS A5.28 (ER80S-D2, ER90S-B3). Flux-cored wires are classified under AWS A5.20 and AWS A5.29 (including seismic self-shielded E71T-8 and low-temp E81T1-Ni1). Submerged arc systems ( AWS A5.17 / A5.23 ) mandate combined wire-flux callouts (e.g., F7A2-EM12K, F8A4-EA2-A2), where active fluxes must be strictly avoided in multi-pass welding to prevent brittle Mn and Si buildup.
AWS A5 Specification Architecture & Procurement Framework
The AWS A5 committee establishes standardized chemical composition, mechanical property, usability, and packaging criteria across all commercial arc welding consumables. For a Certified Welding Engineer (CWEng), understanding consumable specifications extends beyond memorizing classification numbers—it requires managing procurement quality control via AWS A5.01M/A5.01 ( Procurement Guidelines for Consumables - Welding and Allied Processes - Flux and Gas Shielded Electrical Arc Welding ). +-----------------------------------------------------------------------------------------+
- | AWS A5 SPECIFICATION MATRIX FOR CARBON & LOW-ALLOY STEELS |
- +------------------------------------+--------------------------+-------------------------+
- | Welding Process | Carbon Steel Class | Low-Alloy Steel Class |
- +------------------------------------+--------------------------+-------------------------+
- | Shielded Metal Arc Welding (SMAW) | AWS A5.1 / A5.1M | AWS A5.5 / A5.5M |
- | Gas Metal / GTAW (Solid Wire/Rod) | AWS A5.18 / A5.18M | AWS A5.28 / A5.28M |
- | Flux Cored Arc Welding (FCAW) | AWS A5.20 / A5.20M | AWS A5.29 / A5.29M |
- | Submerged Arc Welding (SAW) | AWS A5.17 / A5.17M | AWS A5.23 / A5.23M |
- | Metal Cored Arc Welding (GMAW-C) | AWS A5.18 (or A5.36) | AWS A5.28 (or A5.36) |
- +------------------------------------+--------------------------+-------------------------+
- Quality Verification & Procurement Schedules (AWS A5.01)
When specifying consumables for critical structural (AWS D1.1, AWS D1.8), bridge (AASHTO/AWS D1.5), or pressure containment (ASME Section IX/BPVC Section II Part C) fabrications, the engineer must stipulate testing schedules and lot integrity:
Lot Classifications:
Covered Electrodes (SMAW): Class C1 (manufacturer standard dry blend batch) through Class C5 (strictly controlled chemical and raw material lot).
Solid Wire (GMAW/GTAW/SAW): Class S1 (standard heat lot) through Class S4 (controlled heat plus surface conditioning and chemical testing per spool).
Flux (SAW): Class T1 (standard blend batch) through Class T4 (homogenized production lot).
Testing Schedules:
Schedule F: Manufacturer typical material test certificate (no specific lot testing).
Schedule I: Chemical analysis of the specific lot shipped.
Schedule J: Mechanical testing (all-weld-metal tension and Charpy V-Notch impacts) of the specific lot shipped.
Schedule K: Full chemical, mechanical, radiography, and diffusible hydrogen testing executed on the actual production lot purchased.
AWS A5.1 & AWS A5.5: SMAW Consumables & Coating Metallurgy
Shielded Metal Arc Welding consumables rely on extruded mineral, organic, and metallic flux coverings that perform gas shielding, arc stabilization, slag formation, deoxidation, and alloy transfer. AWS A5.1 SMAW CLASSIFICATION SYNTAX
- E 70 1 8 - H4 R
- | | | | | |
- Electrode Min Tensile Position Coating/Current Diff. Moisture
- (ksi x 1000) 1 = All 8 = Low-H Basic Hydro. Resistant
- 2 = Flat/H Iron Powder <=4mL
- 4 = Vert-Dn /100g
- Core Carbon Steel Electrodes (AWS A5.1)
Classification Coating Type Usability & Current Mechanical Minimums (UTS / YS / %EL / CVN) Engineering Application
E6010 High-Cellulose Sodium All-Position; DCEP only 60 ksi (414 MPa) / 48 ksi (331 MPa) / 22% / 20 ft·lbf @ -20°F (-29°C) Cross-country pipeline root passes (API 1104); aggressive digging arc burns through dirt and rust. High diffusible hydrogen (~30-40 mL/100g).
E6011 High-Cellulose Potassium All-Position; AC or DCEP 60 ksi (414 MPa) / 48 ksi (331 MPa) / 22% / 20 ft·lbf @ -20°F (-29°C) Maintenance and field fabrication where only alternating current (AC) power sources are available.
E7018 / E7018-1 Basic Low-Hydrogen, Iron Powder (25-40%) All-Position; DCEP or AC 70 ksi (483 MPa) / 58 ksi (400 MPa) / 22% / 20 ft·lbf @ -20°F (-29°C) [E7018-1: 20 ft·lbf @ -45°F (-43°C)] Primary structural steel consumable (AWS D1.1); superior fracture toughness and delayed cracking resistance.
E7024 Rutile, High Iron Powder (approx. 50%) Flat and Horizontal Fillet only; AC, DCEP, DCEN 70 ksi (483 MPa) / 58 ksi (400 MPa) / 17% / No mandatory CVN High-speed, heavy fillet production in structural shops; thick slag, fluid pool, zero all-position capability.
AWS A5.5 Low-Alloy Suffix System
AWS A5.5 covers low-alloy SMAW electrodes where precise weld deposit chemistry must match base metal hardenability, creep resistance, cryogenic toughness, or weather-resisting characteristics. Suffix designators define nominal chemistry:
-A1 (Carbon-Molybdenum): 0.5% Mo (nominal). Used for elevated temperature steam piping and boiler tubes (ASTM A204, A335 Gr P1) up to 500°C (930°F).
-B1, -B2, -B3, -B4, -B5 (Chromium-Molybdenum): Creep-resistant alloys:
-B2 : 1.25% Cr – 0.5% Mo (e.g., E8018-B2 for ASTM A387 Gr 11).
-B3 : 2.25% Cr – 1.0% Mo (e.g., E9018-B3 for ASTM A387 Gr 22).
Requires preheat (150°C–250°C) and mandatory Postweld Heat Treatment (PWHT) to temper hard martensitic/bainitic microstructures.
-C1, -C2, -C3 (Nickel Steels): Cryogenic notch toughness:
-C1 : 2.5% Ni (e.g., E8018-C1, CVN >= 20 ft·lbf at -75°F / -59°C).
-C2 : 3.5% Ni (e.g., E8018-C2, CVN >= 20 ft·lbf at -100°F / -73°C).
-C3 : 1.0% Ni, 0.15% Cr, 0.35% Mo (e.g., E8018-C3, CVN >= 20 ft·lbf at -40°F / -40°C), widely used in high-strength structural fabrication.
-D1, -D2, -D3 (Manganese-Molybdenum): 1.25–2.0% Mn, 0.25–0.45% Mo (e.g., E9018-D2 for ASTM A514/A517 quenched and tempered steels).
-M (Military / High Toughness): Formulated for high-yield submarine and defense steels (HY-80, HY-100, HSLA-100). Mandates tight chemical windows, ultra-low diffusible hydrogen (H4 max), and high CVN toughness at -60°F (-51°C) (e.g., E10018-M).
AWS A5.18 & AWS A5.28: GMAW / GTAW Solid Wires & Deoxidation Kinetics
Solid bare wires for Gas Metal Arc Welding (GMAW) and Gas Tungsten Arc Welding (GTAW) rely entirely on internal chemical alloying elements—predominantly manganese (Mn) and silicon (Si)—to scavenge oxygen from the molten weld puddle, preventing carbon monoxide (CO) gas porosity.
Deoxidation Reactions in Steel Weld Pools
Molten iron dissolves atomic oxygen at temperatures above 1538°C. Upon cooling, dissolved oxygen reacts with dissolved carbon: [ C ] + [ O ] ⇌ C O ( g ) [C] + [O] \rightleftharpoons CO_{(g)} [ C ] + [ O ] ⇌ C O ( g )
If CO gas evolves during solidification, severe wormhole and spherical porosity forms. Silicon and manganese deoxidize the weld pool preferentially by forming solid microscopic oxide slags that float to the weld surface: [ S i ] + 2 [ O ] ⇌ S i O 2 ( s ) [Si] + 2[O] \rightleftharpoons SiO_{2(s)} [ S i ] + 2 [ O ] ⇌ S i O 2 ( s ) [ M n ] + [ O ] ⇌ M n O ( s ) [Mn] + [O] \rightleftharpoons MnO_{(s)} [ M n ] + [ O ] ⇌ M n O ( s ) M n O + S i O 2 ⇌ M n S i O 3 ( s ) ( Rhodonite Slag Islands ) MnO + SiO_2 \rightleftharpoons MnSiO_{3(s)} \quad (\text{Rhodonite Slag Islands}) M n O + S i O 2 ⇌ M n S i O 3 ( s ) ( Rhodonite Slag Islands ) AWS A5.18 SOLID WIRE NOMENCLATURE
- ER 70 S - 6
- | | | |
- Electrode or Min Tensile Solid Chemical
- Welding Rod (70 ksi / 483 MPa) Wire Composition
- (High Si-Mn)
- Comparison of Primary AWS A5.18 Carbon Steel Wires
Classification Mn Content (%) Si Content (%) Other Deoxidizers Shielding Gas Compatibility Engineering Characteristics
ER70S-2 0.90 – 1.40 0.40 – 0.70 Ti: 0.05–0.15%; Zr: 0.02–0.12%; Al: 0.05–0.15% 100% Ar (GTAW), Ar/CO2 blends Triple-deoxidized wire. Essential for GTAW root passes in pipe; deoxidizes light rust, oil, and mill scale.
ER70S-3 1.00 – 1.40 0.45 – 0.75 None Ar/CO2 or 100% CO2 Moderate deoxidation; clean sheet metal, automotive, automated manufacturing where mill scale is absent.
ER70S-6 1.40 – 1.85 0.80 – 1.15 None 100% CO2, Ar/CO2 (75/25, 85/15, 90/10) High deoxidation. Yields high fluidity, excellent puddle wetting, flat bead profile, and CVN >= 20 ft·lbf @ -20°F (-29°C). Industry standard.
AWS A5.28 Low-Alloy Solid Wires
ER80S-D2: Alloyed with 1.60–2.10% Mn and 0.40–0.60% Mo. Provides 80 ksi minimum tensile strength with high yield strength (68 ksi min) in both as-welded and stress-relieved conditions; common in heavy crane construction and cross-country pipeline tie-ins.
ER90S-B3: 2.25% Cr – 1.0% Mo solid wire for GTAW/GMAW fabrication of boiler headers and refinery hydrocrackers operating at up to 600°C (1112°F).
AWS A5.20 & AWS A5.29: Flux Cored Arc Welding (FCAW) Consumables
Flux Cored Arc Welding combines continuous wire feeding with internal flux cores that provide gas shielding, arc stabilization, slag formation, and alloy additions. AWS A5.20 FCAW CLASSIFICATION SYNTAX
- E 7 1 T - 1 C / M - J H8
- | | | | | | | | |
- Electrode Tensile Position Tubular Usability Gas Shield CVN Diff. H
- (x10 ksi) 0=Flat/H (Flux) & Slag C = 100% CO2 -40°F <=8mL/100g
- 1=All-Pos Type M = Ar/CO2
Gas-Shielded FCAW-G vs. Self-Shielded FCAW-S +-----------------------------------------------------------------------------------------+
- | FCAW PROCESS COMPARISON MATRIX |
- +------------------------------------+--------------------------+-------------------------+
- | Feature | Gas-Shielded (FCAW-G) | Self-Shielded (FCAW-S) |
- +------------------------------------+--------------------------+-------------------------+
- | AWS Specification | AWS A5.20 / AWS A5.29 | AWS A5.20 / AWS A5.29 |
- | Representative Classifications | E70T-1C, E71T-1M, | E71T-8, E71T-11, |
- | | E81T1-Ni1M | E70T-4 |
- | External Gas Supply | Required (100% CO2 or | None (flux generates |
- | | 75-80% Ar / balance CO2) | internal vapor shield) |
- | Slag Chemistry Type | Rutile (TiO2) or Basic | Fluoride-Aluminate- |
- | | (CaCO3 / CaF2) | Rutile with BaF2/CaF2 |
- | Deoxidation Mechanism | Mn, Si in core | Al, Mg in core |
- | Wind Sensitivity Threshold | > 5 mph (8 km/h) disrupts| Up to 30-35 mph |
- | | gas shield -> porosity | (48-56 km/h) resistant |
- | Primary Industrial Niche | Shop fabrication, heavy | Outdoor civil erection, |
- | | manufacturing, vessels | seismic moment frames |
- +------------------------------------+--------------------------+-------------------------+
- Critical Seismic Performance: AWS D1.8 and E71T-8
In earthquake-resistant structural steel moment frames (governed by AWS D1.8/D1.8M Structural Welding Code - Seismic Supplement ), Demand Critical Welds require strict notch toughness guarantees:
Minimum CVN of 20 ft·lbf at -20°F (-29°C) .
Minimum CVN of 40 ft·lbf at 70°F (+21°C) .
Diffusible hydrogen level H8 or H4 .
E71T-8 electrodes (such as Lincoln Innershield NR-232 / NR-233) are specifically qualified for these seismic moment connections. The core contains metallic aluminum which strips oxygen and nitrogen from the arc, forming fine AlN and Al2O3 precipitates that promote a fine acicular ferrite matrix.
CWEng Metallurgical Alert: Intermixing FCAW-S with Other Processes Self-shielded FCAW-S deposits contain high concentrations of residual aluminum (up to 0.5–0.8% Al). If a weld groove is partially filled with FCAW-S and subsequently capped or back-welded with a gas-shielded process (FCAW-G or GMAW) containing titanium or boron, dilution intermixing triggers brittle coarse carbonitrides and free grain boundary nitrogen. Charpy V-notch toughness plummets from 40 ft·lbf to under 5 ft·lbf! AWS D1.8 Clause 6.4 strictly forbids intermixing FCAW-S with other processes without specific PQR CVN verification.