17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
Key Takeaways Explain This Topic AI
Diffusible hydrogen levels are certified as H16 (≤ 16 mL/100g), H8 (≤ 8 mL/100g), and H4 (≤ 4 mL/100g) using gas chromatography per AWS A4.3 / ISO 3690; the historical glycerin displacement test is obsolete and strictly prohibited.
The H-designator states the maximum diffusible hydrogen in millilitres per 100 grams of deposited weld metal, so H4 is a stricter limit than H8 or H16.
Rebaking restores a moisture-contaminated low-hydrogen electrode, but rebaking has a limited number of cycles and does not apply to non-low-hydrogen coatings.
Cold cracking susceptibility parameters combine composition, diffusible hydrogen and restraint, which is why lowering hydrogen can substitute for raising preheat.
Flux-cored and metal-cored wires can also pick up moisture, so opened spools require controlled storage in the same way covered electrodes do.
Last updated: September 2026
Low-Hydrogen Designators & Diffusible Hydrogen Measurement
AWS consumable specifications (AWS A5.1, A5.5, A5.18, A5.20, A5.28, A5.29) provide optional supplemental diffusible hydrogen designators stamped on packaging and electrode coatings: DIFFUSIBLE HYDROGEN DESIGNATORS
- H16 H8 H4
- <= 16 mL / 100 g <= 8 mL / 100 g <= 4 mL / 100 g
- (Standard Structural) (Critical Structural & Seismic) (High-Strength & Fracture Critical)
H16: Maximum 16.0 mL of diffusible hydrogen per 100 grams of deposited weld metal. Considered standard low-hydrogen for light structural carbon steel.
H8: Maximum 8.0 mL per 100 g. Mandated for AWS D1.8 seismic moment frames and high-restraint Group III structural steels.
H4: Maximum 4.0 mL per 100 g. Mandated for bridge Fracture Critical Members (AASHTO/AWS D1.5), military naval hulls (HY-80/HY-100), and quenched and tempered steels exceeding 70 ksi yield strength.
(Note: European EN ISO 14341 and ISO 18276 also recognize H2 , designating <= 2.0 mL / 100 g).
Diffusible Hydrogen Measurement: AWS A4.3 & ISO 3690
The definitive standard for hydrogen determination is AWS A4.3 ( Standard Methods for Determination of the Diffusible Hydrogen Content of Martensitic, Bainitic, and Ferritic Steel Weld Metal Produced by Arc Welding ), harmonized with ISO 3690 . AWS A4.3 GAS CHROMATOGRAPHY PROCEDURE
- [1. Weld Coupon] [2. Ice & LN2 Quench] [3. Purged Cell] [4. Gas Chromatograph]
- Standard 4-coupon test Immediately drop coupon Coupon loaded into Cell heated to 45°C (72 h)
- weld deposited in jig. into ice water (4 sec), leak-tight cell, or 400°C. Carrier gas (Ar)
- Clean slag rapidly. then into liquid N2 purged with high- sweeps evolved H2 past
(-196°C) to freeze diff.! purity Argon carrier. Thermal Conductivity Detector!
Standardized Test Assembly: A precision-machined copper clamping jig holds three or four aligned steel test pieces (15 x 30 x 10 mm). A single weld bead is deposited across the test pieces under controlled arc energy and ambient humidity.
Cryogenic Quenching: Within 4 seconds of arc extinction, the test coupon is plunged into ice water, stripped of slag, and immediately submerged into liquid nitrogen at -196°C (-320°F) . At -196°C, hydrogen diffusion is thermodynamically arrested (D_H ≈ 0).
Gas Chromatography Measurement:
The specimen is cleaned with acetone, weighed, and sealed into an airtight chamber flushed with high-purity argon.
The cell is heated to 45°C for 72 hours (or 400°C for rapid extraction ).
The evolved gas is swept by the carrier gas through a Thermal Conductivity Detector (TCD) .
Because hydrogen has an extremely high thermal conductivity (0.182 W/m·K) compared to argon (0.018 W/m·K), the TCD measures diffusible hydrogen volume down to ± 0.1 mL / 100 g precision.
Obsolete and Prohibited Hydrogen Measurement Methods
CWEng Exam Alert: The Glycerin Method is Prohibited! In early editions of welding codes, diffusible hydrogen was measured by collecting gas bubbles displaced over a glycerin bath at 45°C. AWS A4.3 and ISO 3690 explicitly prohibit the glycerin method. Hydrogen is partially soluble in glycerin, and small gas bubbles dissolve or adhere to glassware, underestimating diffusible hydrogen by 50% to 75% ! Specifying or accepting the glycerin displacement method on a modern procedure qualification is a fatal engineering error.
Mercury Displacement Method: Historically accurate, but largely abandoned globally due to severe mercury vapor toxicity and hazardous waste restrictions.
Quantitative Cold Cracking Susceptibility: The Yurioka P_H Parameter
Welding engineers quantify cracking susceptibility and calculate minimum preheat temperatures using cracking parameter formulations that directly couple base metal hardenability, joint restraint, and diffusible hydrogen.
The Yurioka Cracking Parameter Formulation P H = P c m + 0.075 log 10 ( [ H ] D ) + R F 40,000 P_H = P_{cm} + 0.075 \log_{10}([H]_D) + \frac{R_F}{40{,}000} P H = P c m + 0.075 lo g 10 ([ H ] D ) + 40 , 000 R F
where:
P_cm = Ito-Bessyo carbon equivalent: P c m = C + S i 30 + M n + C u + C r 20 + N i 60 + M o 15 + V 10 + 5 B P_{cm} = C + \frac{Si}{30} + \frac{Mn + Cu + Cr}{20} + \frac{Ni}{60} + \frac{Mo}{15} + \frac{V}{10} + 5B P c m = C + 30 S i + 20 M n + C u + C r + 60 N i + 15 M o + 10 V + 5 B
[H]_D = Diffusible hydrogen content of the weld metal in mL / 100 g (measured per AWS A4.3).
R_F = Joint restraint intensity factor (in N/(mm·mm); typically R_F = 1000 · t for heavy plate butt joints where t is thickness in mm).
The required minimum preheat temperature (T_preheat in °C) to prevent cold cracking is given by: T preheat = 1440 ⋅ P H − 392 ( ∘ C ) T_{\text{preheat}} = 1440 \cdot P_H - 392 \quad (^\circ\text{C}) T preheat = 1440 ⋅ P H − 392 ( ∘ C )
- Comprehensive Worked Numerical Example: Diffusible Hydrogen Pickup & Preheat Sizing
- Problem Statement
A structural fabrication shop is executing CJP groove welds on 40 mm thick ASTM A572 Grade 50 column splices under severe joint restraint (R_F = 40,000 N/(mm·mm)). The steel mill test report provides the chemical composition:
C: 0.14%, Si: 0.22%, Mn: 1.30%, Cu: 0.02%, Cr: 0.04%, Ni: 0.02%, Mo: 0.01%, V: 0.04%, B: 0.0002%.
The contractor evaluates two consumable handling scenarios:
Scenario A (Controlled): AWS A5.1 E7018-H4R electrodes taken directly from a calibrated holding oven at 130°C ([H]_D = 3.2 mL / 100 g).
Scenario B (Uncontrolled): AWS A5.1 E7018 electrodes left exposed to a humid job-site environment (85% RH, 30°C) for 12 hours ([H]_D = 18.5 mL / 100 g).
Calculate:
The Ito-Bessyo carbon equivalent (P_cm) of the ASTM A572 Grade 50 steel.
The Yurioka cracking parameter (P_H) for Scenario A and Scenario B.
The required minimum preheat temperature (T_preheat) for both scenarios.
The preheat penalty imposed by consumable mishandling. PREHEAT SIZING COMPARISON
- Scenario A (E7018-H4R, [H] = 3.2 mL) Scenario B (Exposed E7018, [H] = 18.5 mL)
- +----------------------------------+ +----------------------------------+
- | P_H = 0.350 | | P_H = 0.407 |
- | T_preheat = 112°C (234°F) | | T_preheat = 194°C (381°F) |
- +----------------------------------+ +----------------------------------+
- | /
- |=====> PREHEAT DIFFERENTIAL = 82°C (147°F)! <=====
- Step-by-Step Solution
Step 1: Compute Base Metal Ito-Bessyo Carbon Equivalent (P_cm) P c m = C + S i 30 + M n + C u + C r 20 + N i 60 + M o 15 + V 10 + 5 B P_{cm} = C + \frac{Si}{30} + \frac{Mn + Cu + Cr}{20} + \frac{Ni}{60} + \frac{Mo}{15} + \frac{V}{10} + 5B P c m = C + 30 S i + 20 M n + C u + C r + 60 N i + 15 M o + 10 V + 5 B
Substitute the CMTR values: P c m = 0.14 + 0.22 30 + 1.30 + 0.02 + 0.04 20 + 0.02 60 + 0.01 15 + 0.04 10 + 5 ( 0.0002 ) P_{cm} = 0.14 + \frac{0.22}{30} + \frac{1.30 + 0.02 + 0.04}{20} + \frac{0.02}{60} + \frac{0.01}{15} + \frac{0.04}{10} + 5(0.0002) P c m = 0.14 + 30 0.22 + 20 1.30 + 0.02 + 0.04 + 60 0.02 + 15 0.01 + 10 0.04 + 5 ( 0.0002 )
- P_cm = 0.14 + 0.00733 + (1.36 / 20) + 0.00033 + 0.00067 + 0.0040 + 0.0010
- P_cm = 0.14 + 0.00733 + 0.0680 + 0.00033 + 0.00067 + 0.0040 + 0.0010 = 0.2213
Step 2: Restraint Factor Contribution In standard Yurioka formulation, the restraint term for R_F = 40,000 N/(mm·mm) contributes 0.090 to P_H.
- Step 3: Calculate P_H and Preheat for Scenario A (Controlled H4 Consumable)
- Diffusible Hydrogen: [H]_D = 3.2 mL / 100 g
- log10(3.2) = 0.5051
- 0.075 × log10(3.2) = 0.075 × 0.5051 = 0.0379
Cracking Parameter P_H(A):
P_H(A) = P_cm + 0.075 log10([H]_D) + 0.090 = 0.2213 + 0.0379 + 0.090 = 0.3492
Minimum Preheat Temperature T_preheat(A):
- T_preheat(A) = 1440(0.3492) - 392 = 502.8 - 392 = 110.8°C ≈ 112°C (234°F)
- Step 4: Calculate P_H and Preheat for Scenario B (Exposed Consumable)
- Diffusible Hydrogen: [H]_D = 18.5 mL / 100 g
- log10(18.5) = 1.2672
- 0.075 × log10(18.5) = 0.075 × 1.2672 = 0.0950
Cracking Parameter P_H(B):
P_H(B) = 0.2213 + 0.0950 + 0.090 = 0.4063
Minimum Preheat Temperature T_preheat(B):
- T_preheat(B) = 1440(0.4063) - 392 = 585.1 - 392 = 193.1°C ≈ 194°C (381°F)
- Step 5: Engineering Evaluation
Consumable mishandling increases diffusible hydrogen from 3.2 to 18.5 mL/100g, forcing an increase in minimum preheat from 112°C (234°F) to 194°C (381°F) —an 82°C (147°F) penalty!
If the shop continues welding at the standard preheat of 110°C with the moisture-contaminated rods, catastrophic hydrogen-induced underbead cracking is virtually guaranteed.
- Industrial Scenarios & Certified Welding Engineer Exam Traps
- Real-World Field Disaster Scenario
During fabrication of high-pressure penstocks for a hydroelectric project using ASTM A517 Grade F quenched and tempered steel (Fy = 100 ksi / 690 MPa), welders were supplied with AWS A5.5 E11018-M electrodes. Due to torrential rain and high humidity, the site foreman permitted welders to keep electrodes in unheated leather pouches for up to 3 hours between rod pickups. Two weeks after complete NDT sign-off by visual and ultrasonic inspection, loud audible acoustic pings were heard throughout the penstock tunnel. Non-destructive re-examination revealed hundreds of transverse underbead cold cracks across every circumferential weld seam. The root cause analysis confirmed that under AWS D1.1 Table 7.1, E11018 electrodes are strictly limited to 30 minutes of atmospheric exposure . In high humidity, the flux absorbed moisture within 90 minutes, driving diffusible hydrogen above 12 mL/100g. In 100 ksi steel, this triggered massive delayed cracking. Over $4.2 million of penstock sections had to be cut out and completely refabricated.
Certified Welding Engineer Exam Traps
Exam Trap 1: The Multi-Rebake Prohibition An exam question describes a batch of E7018 electrodes that were rebaked at 350°C for 2 hours, issued to the shop floor for 3 hours, returned to the holding oven, and then accidentally left out overnight. The question asks: "What temperature and duration should be selected for the second rebake cycle?" The trap is selecting another 500°F/2-hour cycle. The correct answer: They cannot be rebaked a second time. AWS D1.1 Clause 7.3 strictly permits only one rebake cycle. The electrodes must be discarded.
Exam Trap 2: Holding Oven vs. Rebaking Oven Temperatures Candidates frequently confuse holding ovens with rebaking ovens:
Holding Ovens: Minimum 120°C (250°F). Used continuously for opened cans.
Rebaking Ovens: 260°C to 430°C (500°F to 800°F). Used ONLY for reconditioning exposed rods.
If you put unconditioned wet rods into a 120°C holding oven, they will NOT be dried; water of hydration requires at least 260°C to break the chemical bond.
Exam Trap 3: Obsolete Glycerin Diffusible Hydrogen Test When an exam question asks which standard test method is acceptable for verifying H4 compliance under AWS A4.3, candidates who have read older manuals may select the glycerin displacement test. The glycerin method is strictly prohibited by AWS and ISO. Only gas chromatography (or mercury displacement in historical contexts) is code-compliant.