Study guide
5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution
Key Takeaways Explain This Topic AI
The critical cooling time Δt_8/5 governs the solid-state transformation window of austenite into martensite, bainite, or ferrite-pearlite, serving as the primary metric for preventing cold cracking and heat-affected zone (HAZ) embrittlement.
Cooling time through the 800 to 500 degree C range is the single parameter that links a welding procedure to a continuous-cooling-transformation diagram.
Raising preheat lengthens the cooling time far more efficiently than raising heat input, because the cooling rate depends on the difference between peak and initial plate temperature.
Peak temperature falls steeply with distance from the fusion boundary, which is why the coarse-grained heat-affected zone is typically well under a millimetre wide.
Thin-plate (two-dimensional) and thick-plate (three-dimensional) solutions give different dependence on heat input, so choosing the wrong regime is a systematic error rather than a small one.
Last updated: September 2026
Adams Centerline Cooling Rate Formulations
C. M. Adams simplified Rosenthal's complex exponential equations to derive practical engineering expressions for the cooling rate ( R = ∣ d T d t ∣ R = \left| \frac{dT}{dt} \right| R = d t d T ) along the weld centerline at a specified critical temperature T c T_c T c .
3D Cooling Rate (Thick Plate, τ > 0.9 \tau > 0.9 τ > 0.9 ) R 3 D = ∣ d T d t ∣ T c = 2 π k ( T c − T 0 ) 2 H net = 2 π k v ( T c − T 0 ) 2 η V I R_{3D} = \left| \frac{dT}{dt} \right|_{T_c} = \frac{2 \pi k (T_c - T_0)^2}{H_{\text{net}}} = \frac{2 \pi k v (T_c - T_0)^2}{\eta V I} R 3 D = d t d T T c = H net 2 πk ( T c − T 0 ) 2 = η V I 2 πk v ( T c − T 0 ) 2
2D Cooling Rate (Thin Plate, τ < 0.6 \tau < 0.6 τ < 0.6 ) R 2 D = ∣ d T d t ∣ T c = 2 π k ρ C p ( d H net ) 2 ( T c − T 0 ) 3 = 2 π k ρ C p ( v d η V I ) 2 ( T c − T 0 ) 3 R_{2D} = \left| \frac{dT}{dt} \right|_{T_c} = 2 \pi k \rho C_p \left( \frac{d}{H_{\text{net}}} \right)^2 (T_c - T_0)^3 = 2 \pi k \rho C_p \left( \frac{v d}{\eta V I} \right)^2 (T_c - T_0)^3 R 2 D = d t d T T c = 2 πk ρ C p ( H net d ) 2 ( T c − T 0 ) 3 = 2 πk ρ C p ( η V I v d ) 2 ( T c − T 0 ) 3
Comparison of Mathematical Sensitivities
Operational Parameter 3D Thick-Plate Cooling Rate ( R 3 D R_{3D} R 3 D ) Sensitivity 2D Thin-Plate Cooling Rate ( R 2 D R_{2D} R 2 D ) Sensitivity
Net Heat Input ( H net H_{\text{net}} H net ) Inversely proportional: R 3 D ∝ 1 H net R_{3D} \propto \frac{1}{H_{\text{net}}} R 3 D ∝ H net 1 Inversely proportional to the square: R 2 D ∝ 1 H net 2 R_{2D} \propto \frac{1}{H_{\text{net}}^2} R 2 D ∝ H net 2 1
Plate Thickness ( d d d ) Completely independent of thickness d d d Directly proportional to thickness squared: R 2 D ∝ d 2 R_{2D} \propto d^2 R 2 D ∝ d 2
Temperature Difference ( T c − T 0 T_c - T_0 T c − T 0 ) Proportional to squared difference: R 3 D ∝ ( T c − T 0 ) 2 R_{3D} \propto (T_c - T_0)^2 R 3 D ∝ ( T c − T 0 ) 2 Proportional to cubed difference: R 2 D ∝ ( T c − T 0 ) 3 R_{2D} \propto (T_c - T_0)^3 R 2 D ∝ ( T c − T 0 ) 3
Preheat Temperature ( T 0 T_0 T 0 ) Increasing T 0 T_0 T 0 moderately reduces cooling rate Increasing T 0 T_0 T 0 drastically reduces cooling rate
Exam Trap Alert: In 3D heat flow, doubling the plate thickness has zero effect on the weld centerline cooling rate, because heat is already conducting hemispherically into an effectively semi-infinite heat sink. In 2D heat flow, doubling the plate thickness quadruples the cooling rate ( 2 2 = 4 2^2 = 4 2 2 = 4 ) for a fixed heat input per unit length! Do not confuse the two regimes on the CWEng exam.
Critical Cooling Time Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 and Metallurgical Kinetics
In the welding of structural, pressure vessel, and pipeline carbon and low-alloy steels, the single most critical thermal parameter is the cooling time from 800 ∘ C 800^\circ\text{C} 80 0 ∘ C to 500 ∘ C 500^\circ\text{C} 50 0 ∘ C , designated as Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 . Temperature (°C)
- 1000 ┬
- │ Austenite Phase Region
- 800 ┼─────────────────┐ (Start of phase transformation window)
- │ │
- │ │ ◄─── Δt_8/5 (Critical Cooling Time Window)
- │ │
- 500 ┼─────────────────┴ (End of phase transformation window)
- │ Ferrite / Pearlite / Bainite / Martensite Formation
- 200 ┴─────────────────────────────────────────────► Time (s)
- Why the 800 ∘ C → 500 ∘ C 800^\circ\text{C} \to 500^\circ\text{C} 80 0 ∘ C → 50 0 ∘ C Window Dominates
During heating above the A c 3 Ac_3 A c 3 temperature, the base metal transforms to austenite ( γ \gamma γ ). Upon cooling:
Above 800 ∘ C 800^\circ\text{C} 80 0 ∘ C , austenite remains stable; diffusion is rapid, but no structural transformations occur.
Between 800 ∘ C 800^\circ\text{C} 80 0 ∘ C and 500 ∘ C 500^\circ\text{C} 50 0 ∘ C , the austenite decomposes into equilibrium or non-equilibrium microstructures depending on cooling rate (Continuous Cooling Transformation, or CCT, kinetics).
If Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 is too short (excessively fast cooling), carbon cannot diffuse out of the face-centered cubic (FCC) austenite lattice, triggering a diffusionless shear transformation into untempered martensite . Martensite exhibits high hardness, high residual lattice strain, and extreme vulnerability to Hydrogen-Induced Cracking (HIC) / cold cracking.
If Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 is too long (excessively slow cooling), excessive austenite grain growth occurs in the coarse-grained HAZ (CGHAZ), producing coarse upper bainite and ferrite with aligned second phases, leading to severe degradation of Charpy V-notch impact toughness.
Closed-Form Equations for Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5
Integrating Adams cooling formulations across the temperature interval from 800 ∘ C 800^\circ\text{C} 80 0 ∘ C to 500 ∘ C 500^\circ\text{C} 50 0 ∘ C yields:
For 3D Heat Flow (Thick Plate, τ > 0.9 \tau > 0.9 τ > 0.9 ): Δ t 8 / 5 3 D = H net 2 π k [ 1 500 − T 0 − 1 800 − T 0 ] \Delta t_{8/5}^{3D} = \frac{H_{\text{net}}}{2 \pi k} \left[ \frac{1}{500 - T_0} - \frac{1}{800 - T_0} \right] Δ t 8/5 3 D = 2 πk H net [ 500 − T 0 1 − 800 − T 0 1 ]
For 2D Heat Flow (Thin Plate, τ < 0.6 \tau < 0.6 τ < 0.6 ): Δ t 8 / 5 2 D = H net 2 4 π k ρ C p d 2 [ ( 1 500 − T 0 ) 2 − ( 1 800 − T 0 ) 2 ] \Delta t_{8/5}^{2D} = \frac{H_{\text{net}}^2}{4 \pi k \rho C_p d^2} \left[ \left( \frac{1}{500 - T_0} \right)^2 - \left( \frac{1}{800 - T_0} \right)^2 \right] Δ t 8/5 2 D = 4 πk ρ C p d 2 H net 2 [ ( 500 − T 0 1 ) 2 − ( 800 − T 0 1 ) 2 ]
Peak Temperature Distribution T p ( y ) T_p(y) T p ( y ) across the Heat-Affected Zone (HAZ)
The microstructure and mechanical properties across a welded joint vary continuously because each point experiences a distinct thermal cycle characterized by a unique peak temperature ( T p T_p T p ) . Adams formulated expressions relating peak temperature T p T_p T p at a transverse distance y y y from the fusion boundary:
For 2D Thin-Plate Conduction: 1 T p − T 0 = 1 T m − T 0 + 4.13 ρ C p d y H net \frac{1}{T_p - T_0} = \frac{1}{T_m - T_0} + \frac{4.13 \, \rho C_p d \, y}{H_{\text{net}}} T p − T 0 1 = T m − T 0 1 + H net 4.13 ρ C p d y
For 3D Thick-Plate Conduction: 1 T p − T 0 = 1 T m − T 0 + 2 π e ρ C p y 2 H net \frac{1}{T_p - T_0} = \frac{1}{T_m - T_0} + \frac{2 \pi e \, \rho C_p \, y^2}{H_{\text{net}}} T p − T 0 1 = T m − T 0 1 + H net 2 π e ρ C p y 2
where:
T m T_m T m = Liquidus melting temperature of the alloy ( ∘ C ^\circ\text{C} ∘ C ; for carbon steel, ≈ 1530 ∘ C \approx 1530^\circ\text{C} ≈ 153 0 ∘ C )
- y y y = Perpendicular distance from the fusion line into the base metal ( mm \text{mm} mm )
- e = 2.71828 e = 2.71828 e = 2.71828 = Base of the natural logarithm
- The Four Distinct Sub-Zones of the Steel HAZ Fusion Line CGHAZ FGHAZ ICHAZ SCHAZ Unaffected Base Metal
- │ 1100°C-Tm Ac3-1100°C Ac1-Ac3 < Ac1
- │◄─────►│◄──────────►│◄──────────►│◄──────────►│◄───────────►│
- │ Coarse│ Fine │ Partially │ Tempered │ Original Base
- │ Grains│ Equiaxed │ Transformed│ Spheroid- │ Microstructure
- │ Hard/ │ Tough/ │ M-A Islands│ ized │
- │ Brittle Ductile │ Local Soft │ Softened │
Coarse-Grained HAZ (CGHAZ, 1100 ∘ C < T p < T m 1100^\circ\text{C} < T_p < T_m 110 0 ∘ C < T p < T m ): Extreme peak temperatures drive dissolution of grain-pinning precipitates (e.g., Nb(C,N) \text{Nb(C,N)} Nb(C,N) , TiN \text{TiN} TiN ), leading to massive austenite grain growth ( > 100 μ m >100\,\mu\text{m} > 100 μ m ). Upon rapid cooling, it transforms to martensite or coarse upper bainite, presenting the lowest toughness and highest cold cracking risk.
Fine-Grained HAZ (FGHAZ, A c 3 < T p < 1100 ∘ C Ac_3 < T_p < 1100^\circ\text{C} A c 3 < T p < 110 0 ∘ C ): Complete re-austenitization occurs, but lower peak temperatures prevent grain coarsening. Subsequent cooling produces ultra-fine, equiaxed ferrite-pearlite or fine lower bainite, exhibiting optimal impact toughness.
Intercritical HAZ (ICHAZ, A c 1 < T p < A c 3 Ac_1 < T_p < Ac_3 A c 1 < T p < A c 3 ): Partial austenitization occurs within the two-phase ferrite + austenite field. Carbon partitions preferentially into the austenite islands, which upon rapid cooling transform into hard, brittle Martensite-Austenite (M-A) constituents , creating localized brittle zones (LBZs).
Subcritical HAZ (SCHAZ, T p < A c 1 T_p < Ac_1 T p < A c 1 ): Peak temperatures remain below the lower transformation temperature. No phase changes occur, but existing base metal carbides or cold-worked grains undergo tempering, recovery, and localized softening.
- Comprehensive Worked Numerical Example: Complete Thermal Profile
- Problem Statement
A heavy structural girder fabricated from ASTM A572 Grade 50 steel plate with thickness d = 35.0 mm d = 35.0\text{ mm} d = 35.0 mm is joined using Submerged Arc Welding (SAW). The welding procedure operates under the following conditions:
- Arc Voltage V = 30.0 V V = 30.0\text{ V} V = 30.0 V
- Welding Current I = 500.0 A I = 500.0\text{ A} I = 500.0 A
- Travel Speed v = 6.0 mm/s v = 6.0\text{ mm/s} v = 6.0 mm/s ( 360 mm/min 360\text{ mm/min} 360 mm/min )
- Initial Workpiece Preheat T 0 = 50.0 ∘ C T_0 = 50.0^\circ\text{C} T 0 = 50. 0 ∘ C
- Arc Thermal Efficiency η = 0.95 \eta = 0.95 η = 0.95 (typical SAW process)
- Liquidus Melting Temperature T m = 1530.0 ∘ C T_m = 1530.0^\circ\text{C} T m = 1530. 0 ∘ C
Material Properties:
Thermal Conductivity k = 40.0 W/(m ⋅ K) = 0.040 J/(mm ⋅ s ⋅ ∘ C) k = 40.0\text{ W/(m}\cdot\text{K)} = 0.040\text{ J/(mm}\cdot\text{s}\cdot^\circ\text{C)} k = 40.0 W/(m ⋅ K) = 0.040 J/(mm ⋅ s ⋅ ∘ C)
Volumetric Heat Capacity ρ C p = 4.50 × 10 6 J/(m 3 ⋅ K) = 0.00450 J/(mm 3 ⋅ ∘ C) \rho C_p = 4.50 \times 10^6\text{ J/(m}^3\cdot\text{K)} = 0.00450\text{ J/(mm}^3\cdot^\circ\text{C)} ρ C p = 4.50 × 1 0 6 J/(m 3 ⋅ K) = 0.00450 J/(mm 3 ⋅ ∘ C)
Thermal Diffusivity α = 8.89 mm 2 / s \alpha = 8.89\text{ mm}^2/\text{s} α = 8.89 mm 2 / s
Calculate:
The gross and net heat inputs per unit length ( H gross H_{\text{gross}} H gross and H net H_{\text{net}} H net ).
The relative plate thickness τ \tau τ at critical temperature T c = 540 ∘ C T_c = 540^\circ\text{C} T c = 54 0 ∘ C to establish the heat flow regime (2D vs. 3D).
The cooling rate R R R at the weld centerline at T c = 540 ∘ C T_c = 540^\circ\text{C} T c = 54 0 ∘ C .
The critical cooling time Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 .
The peak temperature T p T_p T p at a transverse distance y = 5.0 mm y = 5.0\text{ mm} y = 5.0 mm from the fusion boundary.
Step-by-Step Solution
Step 1: Calculate Gross and Net Heat Input H gross = V ⋅ I v = 30.0 V × 500.0 A 6.0 mm/s = 15 , 000 W 6.0 mm/s = 2500.0 J/mm = 2.50 kJ/mm H_{\text{gross}} = \frac{V \cdot I}{v} = \frac{30.0\text{ V} \times 500.0\text{ A}}{6.0\text{ mm/s}} = \frac{15,000\text{ W}}{6.0\text{ mm/s}} = 2500.0\text{ J/mm} = 2.50\text{ kJ/mm} H gross = v V ⋅ I = 6.0 mm/s 30.0 V × 500.0 A = 6.0 mm/s 15 , 000 W = 2500.0 J/mm = 2.50 kJ/mm H net = η ⋅ H gross = 0.95 × 2500.0 J/mm = 2375.0 J/mm = 2.375 kJ/mm = 2 , 375 , 000 J/m H_{\text{net}} = \eta \cdot H_{\text{gross}} = 0.95 \times 2500.0\text{ J/mm} = 2375.0\text{ J/mm} = 2.375\text{ kJ/mm} = 2,375,000\text{ J/m} H net = η ⋅ H gross = 0.95 × 2500.0 J/mm = 2375.0 J/mm = 2.375 kJ/mm = 2 , 375 , 000 J/m
Step 2: Determine Relative Plate Thickness τ \tau τ (2D vs. 3D Regime) τ = d ρ C p ( T c − T 0 ) H net \tau = d \sqrt{\frac{\rho C_p (T_c - T_0)}{H_{\text{net}}}} τ = d H net ρ C p ( T c − T 0 )
Using SI units: d = 0.035 m d = 0.035\text{ m} d = 0.035 m , ρ C p = 4.50 × 10 6 J/(m 3 ⋅ K) \rho C_p = 4.50 \times 10^6\text{ J/(m}^3\cdot\text{K)} ρ C p = 4.50 × 1 0 6 J/(m 3 ⋅ K) , T c − T 0 = 540 − 50 = 490 ∘ C T_c - T_0 = 540 - 50 = 490^\circ\text{C} T c − T 0 = 540 − 50 = 49 0 ∘ C , H net = 2.375 × 10 6 J/m H_{\text{net}} = 2.375 \times 10^6\text{ J/m} H net = 2.375 × 1 0 6 J/m . ρ C p ( T c − T 0 ) H net = 4.50 × 10 6 × 490 2.375 × 10 6 = 2.205 × 10 9 2.375 × 10 6 = 928.42 m − 2 \frac{\rho C_p (T_c - T_0)}{H_{\text{net}}} = \frac{4.50 \times 10^6 \times 490}{2.375 \times 10^6} = \frac{2.205 \times 10^9}{2.375 \times 10^6} = 928.42\text{ m}^{-2} H net ρ C p ( T c − T 0 ) = 2.375 × 1 0 6 4.50 × 1 0 6 × 490 = 2.375 × 1 0 6 2.205 × 1 0 9 = 928.42 m − 2 928.42 m − 2 = 30.47 m − 1 \sqrt{928.42\text{ m}^{-2}} = 30.47\text{ m}^{-1} 928.42 m − 2 = 30.47 m − 1 τ = 0.035 m × 30.47 m − 1 = 1.066 \tau = 0.035\text{ m} \times 30.47\text{ m}^{-1} = 1.066 τ = 0.035 m × 30.47 m − 1 = 1.066
Evaluation: Since τ = 1.066 > 0.9 \tau = 1.066 > 0.9 τ = 1.066 > 0.9 , the weldment exhibits unambiguous three-dimensional (3D) thick-plate heat flow . Thermal conduction proceeds hemispherically into the thickness without experiencing thermal reflection from the plate bottom.
Step 3: Calculate 3D Weld Centerline Cooling Rate at T c = 540 ∘ C T_c = 540^\circ\text{C} T c = 54 0 ∘ C Using Adams 3D cooling rate equation: R 3 D = 2 π k ( T c − T 0 ) 2 H net R_{3D} = \frac{2 \pi k (T_c - T_0)^2}{H_{\text{net}}} R 3 D = H net 2 πk ( T c − T 0 ) 2
Substitute values in consistent units ( mm , s , ∘ C \text{mm}, \text{s}, ^\circ\text{C} mm , s , ∘ C ):
- k = 0.040 J/(mm ⋅ s ⋅ ∘ C) k = 0.040\text{ J/(mm}\cdot\text{s}\cdot^\circ\text{C)} k = 0.040 J/(mm ⋅ s ⋅ ∘ C)
- T c − T 0 = 540 − 50 = 490 ∘ C T_c - T_0 = 540 - 50 = 490^\circ\text{C} T c − T 0 = 540 − 50 = 49 0 ∘ C
H net = 2375.0 J/mm H_{\text{net}} = 2375.0\text{ J/mm} H net = 2375.0 J/mm ( T c − T 0 ) 2 = ( 490 ) 2 = 240 , 100 ( ∘ C) 2 (T_c - T_0)^2 = (490)^2 = 240,100\text{ (}^\circ\text{C)}^2 ( T c − T 0 ) 2 = ( 490 ) 2 = 240 , 100 ( ∘ C) 2 R 3 D = 2 × π × 0.040 × 240 , 100 2375.0 = 60 , 343.89 2375.0 = 25.41 ∘ C/s R_{3D} = \frac{2 \times \pi \times 0.040 \times 240,100}{2375.0} = \frac{60,343.89}{2375.0} = 25.41^\circ\text{C/s} R 3 D = 2375.0 2 × π × 0.040 × 240 , 100 = 2375.0 60 , 343.89 = 25.4 1 ∘ C/s
Step 4: Calculate Critical Cooling Time Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 Using the 3D thick-plate formulation: Δ t 8 / 5 3 D = H net 2 π k [ 1 500 − T 0 − 1 800 − T 0 ] \Delta t_{8/5}^{3D} = \frac{H_{\text{net}}}{2 \pi k} \left[ \frac{1}{500 - T_0} - \frac{1}{800 - T_0} \right] Δ t 8/5 3 D = 2 πk H net [ 500 − T 0 1 − 800 − T 0 1 ] H net 2 π k = 2375.0 2 × π × 0.040 = 2375.0 0.251327 = 9449.83 s ⋅ ∘ C \frac{H_{\text{net}}}{2 \pi k} = \frac{2375.0}{2 \times \pi \times 0.040} = \frac{2375.0}{0.251327} = 9449.83\text{ s}\cdot^\circ\text{C} 2 πk H net = 2 × π × 0.040 2375.0 = 0.251327 2375.0 = 9449.83 s ⋅ ∘ C 1 500 − 50 − 1 800 − 50 = 1 450 − 1 750 = 0.0022222 − 0.0013333 = 0.0008889 ∘ C − 1 \frac{1}{500 - 50} - \frac{1}{800 - 50} = \frac{1}{450} - \frac{1}{750} = 0.0022222 - 0.0013333 = 0.0008889\text{ }^\circ\text{C}^{-1} 500 − 50 1 − 800 − 50 1 = 450 1 − 750 1 = 0.0022222 − 0.0013333 = 0.0008889 ∘ C − 1 Δ t 8 / 5 3 D = 9449.83 × 0.0008889 = 8.40 seconds \Delta t_{8/5}^{3D} = 9449.83 \times 0.0008889 = 8.40\text{ seconds} Δ t 8/5 3 D = 9449.83 × 0.0008889 = 8.40 seconds
Step 5: Calculate Peak Temperature at y = 5.0 mm y = 5.0\text{ mm} y = 5.0 mm from Fusion Boundary Using the Adams 3D peak temperature distribution equation: 1 T p − T 0 = 1 T m − T 0 + 2 π e ρ C p y 2 H net \frac{1}{T_p - T_0} = \frac{1}{T_m - T_0} + \frac{2 \pi e \, \rho C_p \, y^2}{H_{\text{net}}} T p − T 0 1 = T m − T 0 1 + H net 2 π e ρ C p y 2 1 T m − T 0 = 1 1530 − 50 = 1 1480 = 6.7568 × 10 − 4 ∘ C − 1 \frac{1}{T_m - T_0} = \frac{1}{1530 - 50} = \frac{1}{1480} = 6.7568 \times 10^{-4}\text{ }^\circ\text{C}^{-1} T m − T 0 1 = 1530 − 50 1 = 1480 1 = 6.7568 × 1 0 − 4 ∘ C − 1 2 π e ρ C p y 2 = 2 × 3.14159 × 2.71828 × 0.00450 × ( 5.0 ) 2 = 17.0795 × 0.00450 × 25.0 = 1.9214 J/(mm ⋅ ∘ C) 2 \pi e \, \rho C_p \, y^2 = 2 \times 3.14159 \times 2.71828 \times 0.00450 \times (5.0)^2 = 17.0795 \times 0.00450 \times 25.0 = 1.9214\text{ J/(mm}\cdot^\circ\text{C)} 2 π e ρ C p y 2 = 2 × 3.14159 × 2.71828 × 0.00450 × ( 5.0 ) 2 = 17.0795 × 0.00450 × 25.0 = 1.9214 J/(mm ⋅ ∘ C) 1.9214 H net = 1.9214 2375.0 = 8.0901 × 10 − 4 ∘ C − 1 \frac{1.9214}{H_{\text{net}}} = \frac{1.9214}{2375.0} = 8.0901 \times 10^{-4}\text{ }^\circ\text{C}^{-1} H net 1.9214 = 2375.0 1.9214 = 8.0901 × 1 0 − 4 ∘ C − 1 1 T p − T 0 = 6.7568 × 10 − 4 + 8.0901 × 10 − 4 = 1.4847 × 10 − 3 ∘ C − 1 \frac{1}{T_p - T_0} = 6.7568 \times 10^{-4} + 8.0901 \times 10^{-4} = 1.4847 \times 10^{-3}\text{ }^\circ\text{C}^{-1} T p − T 0 1 = 6.7568 × 1 0 − 4 + 8.0901 × 1 0 − 4 = 1.4847 × 1 0 − 3 ∘ C − 1 T p − T 0 = 1 1.4847 × 10 − 3 = 673.54 ∘ C T_p - T_0 = \frac{1}{1.4847 \times 10^{-3}} = 673.54^\circ\text{C} T p − T 0 = 1.4847 × 1 0 − 3 1 = 673.5 4 ∘ C T p = 673.54 + 50.0 = 723.5 ∘ C T_p = 673.54 + 50.0 = 723.5^\circ\text{C} T p = 673.54 + 50.0 = 723. 5 ∘ C
Metallurgical Conclusion: At y = 5.0 mm y = 5.0\text{ mm} y = 5.0 mm , T p = 723.5 ∘ C T_p = 723.5^\circ\text{C} T p = 723. 5 ∘ C , which falls just below the lower transformation temperature A c 1 ≈ 727 ∘ C Ac_1 \approx 727^\circ\text{C} A c 1 ≈ 72 7 ∘ C . This location resides in the Subcritical Heat-Affected Zone (SCHAZ) , undergoing carbide tempering without austenite phase re-transformation.
- Real-World Engineering Scenarios & Exam Pitfalls
- Industrial Case: Hydrogen-Induced Cold Cracking in Offshore Monopiles
During the fabrication of thick-walled ( d = 65 mm d = 65\text{ mm} d = 65 mm ) S355ML structural steel offshore wind turbine monopiles, ultrasonic testing revealed extensive transverse cracking in the coarse-grained HAZ within 24 hours of welding. The welding engineer discovered that shop personnel omitted the mandated 125 ∘ C 125^\circ\text{C} 12 5 ∘ C preheat because the ambient shop temperature was 20 ∘ C 20^\circ\text{C} 2 0 ∘ C . Calculating the thermal cycle revealed that without preheat, τ = 65 × 10 − 3 4.5 × 10 6 × ( 540 − 20 ) / 2.0 × 10 6 = 2.22 \tau = 65 \times 10^{-3} \sqrt{4.5 \times 10^6 \times (540 - 20) / 2.0 \times 10^6} = 2.22 τ = 65 × 1 0 − 3 4.5 × 1 0 6 × ( 540 − 20 ) /2.0 × 1 0 6 = 2.22 (deep 3D conduction). The 3D cooling time Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 dropped from 12.8 s 12.8\text{ s} 12.8 s (with preheat) to 4.9 s 4.9\text{ s} 4.9 s (without preheat). This ultra-fast quench transformed the CGHAZ into hard untempered martensite ( 385 HV10 385\text{ HV10} 385 HV10 ), which, combined with weld residual stress and diffusible hydrogen from flux moisture, caused catastrophic cold cracking. Reinstating preheat extended Δ t 8 / 5 \Delta t_{8/5} Δ t 8/5 above 11.0 s 11.0\text{ s} 11.0 s , capping hardness at 270 HV10 270\text{ HV10} 270 HV10 and eliminating cracking.
Common Exam Traps
Exam Trap 1: Conflating Gross Heat Input with Net Heat Input Always check whether a question provides arc efficiency η \eta η . If given, H net = η V I / v H_{\text{net}} = \eta V I / v H net = η V I / v . Rosenthal and Adams cooling formulations rely strictly on net heat input ( H net H_{\text{net}} H net ). Substituting gross heat input ( V I / v V I / v V I / v ) will underestimate cooling rates by 10 % − 35 % 10\% - 35\% 10% − 35% , leading to non-conservative engineering errors.
Exam Trap 2: Applying the 2D Equation to Thick Plates A classic examination error is automatically using the 2D cooling rate equation because it explicitly includes plate thickness d d d . Remember: for τ > 0.9 \tau > 0.9 τ > 0.9 , the plate acts as a semi-infinite 3D heat sink, and cooling rate is completely independent of thickness ! Only when τ < 0.6 \tau < 0.6 τ < 0.6 does thickness enter the equation ( R ∝ d 2 R \propto d^2 R ∝ d 2 ).
Exam Trap 3: Mixing Thermal Conductivity and Thermal Diffusivity Units Thermal conductivity k k k is expressed in W/(m ⋅ K) \text{W/(m}\cdot\text{K)} W/(m ⋅ K) or J/(mm ⋅ s ⋅ ∘ C) \text{J/(mm}\cdot\text{s}\cdot^\circ\text{C)} J/(mm ⋅ s ⋅ ∘ C) , while thermal diffusivity α = k / ( ρ C p ) \alpha = k/(\rho C_p) α = k / ( ρ C p ) is expressed in m 2 / s \text{m}^2/\text{s} m 2 / s or mm 2 / s \text{mm}^2/\text{s} mm 2 / s . When evaluating the exponential terms in Rosenthal's solution ( v / 2 α v/2\alpha v /2 α ), verify that travel speed v v v and diffusivity α \alpha α share identical length units (e.g., mm/s \text{mm/s} mm/s and mm 2 / s \text{mm}^2/\text{s} mm 2 / s ).