Study guide
6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution
Key Takeaways Explain This Topic AI
Resistive heating rises with the square of current, so a modest current increase produces a disproportionate rise in cable and connection losses.
Electrode extension preheating raises melt-off rate at constant current, which is why contact-tip-to-work distance is an essential variable for wire processes.
Voltage measured at the power source includes cable and connection drops, so procedure voltage must be read at or referenced to the arc.
A hot connection or cable is a diagnostic symptom: the lost voltage is no longer available at the arc and the procedure is no longer running as written.
Last updated: September 2026
4. Joule's First Law and Electrode Stickout Resistive Preheating
Joule's First Law defines the rate at which electrical energy is irreversibly converted into thermal energy within a resistive conductor: P = I 2 R = V 2 R P = I^2 R = \frac{V^2}{R} P = I 2 R = R V 2 Q = ∫ 0 t I 2 R d t = I 2 R t ( for constant I , R ) Q = \int_0^t I^2 R \, dt = I^2 R t \quad (\text{for constant } I, R) Q = ∫ 0 t I 2 R d t = I 2 Rt ( for constant I , R )
Parasitic Joule Losses in Welding Cables
Welding cables carry massive currents ( 200 to 600 + A 200\text{ to }600+\text{ A} 200 to 600 + A ). If cables are undersized or excessively long, parasitic Joule losses ( I 2 R cable I^2 R_{\text{cable}} I 2 R cable ) cause:
Severe terminal voltage drop, starving the arc and destabilizing metal transfer.
Thermal degradation of cable insulation (standard synthetic rubber is rated for 60 ∘ C , 75 ∘ C , or 90 ∘ C 60^\circ\text{C}, 75^\circ\text{C},\text{ or }90^\circ\text{C} 6 0 ∘ C , 7 5 ∘ C , or 9 0 ∘ C ).
Runaway resistance growth: copper has a positive temperature coefficient of resistance ( α Cu ≈ + 0.00393 / ∘ C \alpha_{\text{Cu}} \approx +0.00393 / ^\circ\text{C} α Cu ≈ + 0.00393 / ∘ C ), such that heating from 20 ∘ C 20^\circ\text{C} 2 0 ∘ C to 80 ∘ C 80^\circ\text{C} 8 0 ∘ C increases cable resistance by 23.6 % 23.6\% 23.6% , further compounding voltage drop.
Contact Tip Interface Resistance
The electrical contact between the copper alloy contact tip and the advancing electrode wire occurs across microscopic asperities. Sliding contact resistance ( R ct R_{\text{ct}} R ct ) typically ranges from 2 to 8 m Ω 2\text{ to }8\text{ m}\Omega 2 to 8 m Ω in new tips, but escalates above 30 m Ω 30\text{ m}\Omega 30 m Ω as the bore erodes oval from mechanical wear and micro-arcing. This produces local Joule overheating, micro-fusing of the wire inside the bore (burnback), and erratic feeding.
Functional Joule Heating: Wire Extension (Stickout) Preheating
In continuous wire processes (GMAW, FCAW, SAW), the electrode extension ( L ext L_{\text{ext}} L ext , or stickout) is the length of unmelted filler wire projecting beyond the contact tip to the arc. Contact Tip
- +---------+
- | Copper | Wire Feed Speed (v_w)
- | Alloy | =====>
- +----+----+-----------------------------------
- | | Electrode Wire (ER70S-6, Dia d) |
- | | | <-- Resistive Preheating Zone
- +----+-----------------------------------+ (Joule Heating: Q = I^2 * R_ext * t)
- |<----------- L_ext --------------->|
- +--/--- Weld Pool
- | ARC |
The total melting rate of a continuous consumable electrode is expressed by the fundamental Lesnewich equation: MR = α I + β L ext I 2 \text{MR} = \alpha I + \beta L_{\text{ext}} I^2 MR = α I + β L ext I 2
where:
α I \alpha I α I represents arc heating at the cathode or anode fall region ( [ kg / ( h ⋅ A ) ] [\text{kg}/(\text{h}\cdot\text{A})] [ kg / ( h ⋅ A )] ).
β L ext I 2 \beta L_{\text{ext}} I^2 β L ext I 2 represents Joule resistance preheating along the length of the extension ( [ kg / ( h ⋅ mm ⋅ A 2 ) ] [\text{kg}/(\text{h}\cdot\text{mm}\cdot\text{A}^2)] [ kg / ( h ⋅ mm ⋅ A 2 )] ).
The temperature rise Δ T \Delta T Δ T of the wire solid mass before it reaches the arc is: Δ T = ρ e L ext I 2 A 2 ⋅ v w ⋅ ρ m ⋅ c p \Delta T = \frac{\rho_e L_{\text{ext}} I^2}{A^2 \cdot v_w \cdot \rho_m \cdot c_p} Δ T = A 2 ⋅ v w ⋅ ρ m ⋅ c p ρ e L ext I 2
where ρ e \rho_e ρ e is electrical resistivity, A A A is wire cross-sectional area, v w v_w v w is wire feed speed, ρ m \rho_m ρ m is metal density, and c p c_p c p is specific heat capacity.
Increasing stickout increases R ext R_{\text{ext}} R ext , preheating the wire to over 800 ∘ C − 1000 ∘ C 800^\circ\text{C}-1000^\circ\text{C} 80 0 ∘ C − 100 0 ∘ C before it reaches the arc. Consequently, less arc energy is required to complete fusion, allowing dramatic increases in deposition rate at fixed current, or requiring lower current to melt wire at a fixed wire feed speed.
- 5. Comprehensive Worked Numerical Example: Welding Circuit Voltage Distribution & Stickout Preheating
- Problem Statement
A robotic GMAW cell operates with an AWS A5.18 ER70S-6 solid steel wire of diameter d = 1.20 mm d = 1.20\text{ mm} d = 1.20 mm ( 0.00120 m 0.00120\text{ m} 0.00120 m ) at a welding current I = 320 A I = 320\text{ A} I = 320 A DC. The power supply terminal voltage is maintained at V source = 32.0 V V_{\text{source}} = 32.0\text{ V} V source = 32.0 V .
The circuit parameters are:
Total welding cable run: 25.0 m 25.0\text{ m} 25.0 m electrode lead + 25.0 m 25.0\text{ m} 25.0 m work return lead ( L cable = 50.0 m L_{\text{cable}} = 50.0\text{ m} L cable = 50.0 m total) of 2/0 AWG stranded copper cable. Resistance is 0.260 m Ω / m 0.260\text{ m}\Omega/\text{m} 0.260 m Ω/ m at operating temperature ( R cable = 0.0130 Ω R_{\text{cable}} = 0.0130\ \Omega R cable = 0.0130 Ω ).
Contact tip sliding interface resistance: R ct = 5.0 m Ω = 0.0050 Ω R_{\text{ct}} = 5.0\text{ m}\Omega = 0.0050\ \Omega R ct = 5.0 m Ω = 0.0050 Ω .
Ground clamp-to-workpiece contact resistance: R clamp = 4.0 m Ω = 0.0040 Ω R_{\text{clamp}} = 4.0\text{ m}\Omega = 0.0040\ \Omega R clamp = 4.0 m Ω = 0.0040 Ω .
Base metal plate resistance: negligible ( R work ≈ 0 R_{\text{work}} \approx 0 R work ≈ 0 ).
Electrode extension (stickout): L ext = 20.0 mm = 0.020 m L_{\text{ext}} = 20.0\text{ mm} = 0.020\text{ m} L ext = 20.0 mm = 0.020 m .
Average effective electrical resistivity of the steel wire over its preheat range: ρ e = 7.50 × 10 − 7 Ω ⋅ m \rho_e = 7.50 \times 10^{-7}\ \Omega\cdot\text{m} ρ e = 7.50 × 1 0 − 7 Ω ⋅ m .
Wire Feed Speed: W F S = 10.0 m/min = 0.1667 m/s WFS = 10.0\text{ m/min} = 0.1667\text{ m/s} W FS = 10.0 m/min = 0.1667 m/s .
Steel physical properties: density ρ m = 7850 kg/m 3 \rho_m = 7850\text{ kg/m}^3 ρ m = 7850 kg/m 3 , specific heat c p = 620 J/(kg ⋅ ∘ C) c_p = 620\text{ J/(kg}\cdot^\circ\text{C)} c p = 620 J/(kg ⋅ ∘ C) .
Calculate:
The electrical resistance of the wire extension ( R ext R_{\text{ext}} R ext ).
The total series resistance of all circuit components excluding the arc ( R loop R_{\text{loop}} R loop ).
The total parasitic/resistive voltage drop across all components ( V drops V_{\text{drops}} V drops ).
The actual voltage available across the welding arc ( V arc V_{\text{arc}} V arc ).
The power dissipated as waste heat in cables and connections versus power utilized in the arc.
The temperature rise ( Δ T \Delta T Δ T ) of the electrode wire from Joule preheating upon entering the arc.
Step-by-Step Solution
Step 1: Compute wire cross-sectional area and extension resistance ( R ext R_{\text{ext}} R ext ) A = π d 2 4 = π ( 0.00120 m ) 2 4 = 1.131 × 10 − 6 m 2 A = \frac{\pi d^2}{4} = \frac{\pi (0.00120\text{ m})^2}{4} = 1.131 \times 10^{-6}\text{ m}^2 A = 4 π d 2 = 4 π ( 0.00120 m ) 2 = 1.131 × 1 0 − 6 m 2 R ext = ρ e L ext A = ( 7.50 × 10 − 7 Ω ⋅ m ) ( 0.020 m ) 1.131 × 10 − 6 m 2 = 0.01326 Ω = 13.26 m Ω R_{\text{ext}} = \frac{\rho_e L_{\text{ext}}}{A} = \frac{(7.50 \times 10^{-7}\ \Omega\cdot\text{m})(0.020\text{ m})}{1.131 \times 10^{-6}\text{ m}^2} = 0.01326\ \Omega = 13.26\text{ m}\Omega R ext = A ρ e L ext = 1.131 × 1 0 − 6 m 2 ( 7.50 × 1 0 − 7 Ω ⋅ m ) ( 0.020 m ) = 0.01326 Ω = 13.26 m Ω
Step 2: Calculate total non-arc series loop resistance ( R loop R_{\text{loop}} R loop ) R loop = R cable + R ct + R ext + R clamp R_{\text{loop}} = R_{\text{cable}} + R_{\text{ct}} + R_{\text{ext}} + R_{\text{clamp}} R loop = R cable + R ct + R ext + R clamp R loop = 0.0130 Ω + 0.0050 Ω + 0.01326 Ω + 0.0040 Ω = 0.03526 Ω = 35.26 m Ω R_{\text{loop}} = 0.0130\ \Omega + 0.0050\ \Omega + 0.01326\ \Omega + 0.0040\ \Omega = 0.03526\ \Omega = 35.26\text{ m}\Omega R loop = 0.0130 Ω + 0.0050 Ω + 0.01326 Ω + 0.0040 Ω = 0.03526 Ω = 35.26 m Ω
Step 3: Calculate total parasitic voltage drop ( V drops V_{\text{drops}} V drops ) V drops = I ⋅ R loop = 320 A × 0.03526 Ω = 11.28 V V_{\text{drops}} = I \cdot R_{\text{loop}} = 320\text{ A} \times 0.03526\ \Omega = 11.28\text{ V} V drops = I ⋅ R loop = 320 A × 0.03526 Ω = 11.28 V
Individual voltage drops:
Cables: V cable = 320 × 0.0130 = 4.16 V V_{\text{cable}} = 320 \times 0.0130 = 4.16\text{ V} V cable = 320 × 0.0130 = 4.16 V
Contact tip: V ct = 320 × 0.0050 = 1.60 V V_{\text{ct}} = 320 \times 0.0050 = 1.60\text{ V} V ct = 320 × 0.0050 = 1.60 V
Stickout: V ext = 320 × 0.01326 = 4.24 V V_{\text{ext}} = 320 \times 0.01326 = 4.24\text{ V} V ext = 320 × 0.01326 = 4.24 V
Ground clamp: V clamp = 320 × 0.0040 = 1.28 V V_{\text{clamp}} = 320 \times 0.0040 = 1.28\text{ V} V clamp = 320 × 0.0040 = 1.28 V
Step 4: Determine actual arc voltage ( V arc V_{\text{arc}} V arc ) Applying Kirchhoff's Voltage Law: V arc = V source − V drops = 32.00 V − 11.28 V = 20.72 V V_{\text{arc}} = V_{\text{source}} - V_{\text{drops}} = 32.00\text{ V} - 11.28\text{ V} = 20.72\text{ V} V arc = V source − V drops = 32.00 V − 11.28 V = 20.72 V
Step 5: Power distribution breakdown
Total electrical power from source: P total = V source ⋅ I = 32.0 V × 320 A = 10 , 240 W = 10.24 kW P_{\text{total}} = V_{\text{source}} \cdot I = 32.0\text{ V} \times 320\text{ A} = 10,240\text{ W} = 10.24\text{ kW} P total = V source ⋅ I = 32.0 V × 320 A = 10 , 240 W = 10.24 kW
Arc thermal power: P arc = V arc ⋅ I = 20.72 V × 320 A = 6 , 630.4 W P_{\text{arc}} = V_{\text{arc}} \cdot I = 20.72\text{ V} \times 320\text{ A} = 6,630.4\text{ W} P arc = V arc ⋅ I = 20.72 V × 320 A = 6 , 630.4 W ( 64.75 % 64.75\% 64.75% of total power)
Stickout preheating power: P ext = I 2 R ext = ( 320 ) 2 × 0.01326 = 1 , 357.8 W P_{\text{ext}} = I^2 R_{\text{ext}} = (320)^2 \times 0.01326 = 1,357.8\text{ W} P ext = I 2 R ext = ( 320 ) 2 × 0.01326 = 1 , 357.8 W ( 13.26 % 13.26\% 13.26% )
Waste heat in cables: P cable = I 2 R cable = ( 320 ) 2 × 0.0130 = 1 , 331.2 W P_{\text{cable}} = I^2 R_{\text{cable}} = (320)^2 \times 0.0130 = 1,331.2\text{ W} P cable = I 2 R cable = ( 320 ) 2 × 0.0130 = 1 , 331.2 W ( 13.00 % 13.00\% 13.00% )
Waste heat in contact tip: P ct = ( 320 ) 2 × 0.0050 = 512.0 W P_{\text{ct}} = (320)^2 \times 0.0050 = 512.0\text{ W} P ct = ( 320 ) 2 × 0.0050 = 512.0 W ( 5.00 % 5.00\% 5.00% )
Waste heat in ground clamp: P clamp = ( 320 ) 2 × 0.0040 = 409.6 W P_{\text{clamp}} = (320)^2 \times 0.0040 = 409.6\text{ W} P clamp = ( 320 ) 2 × 0.0040 = 409.6 W ( 4.00 % 4.00\% 4.00% )
Step 6: Compute temperature rise of wire from Joule preheating Compute mass flow rate of wire ( m ˙ \dot{m} m ˙ ): m ˙ = A ⋅ v w ⋅ ρ m = ( 1.131 × 10 − 6 m 2 ) × ( 0.1667 m/s ) × ( 7850 kg/m 3 ) = 1.480 × 10 − 3 kg/s \dot{m} = A \cdot v_w \cdot \rho_m = (1.131 \times 10^{-6}\text{ m}^2) \times (0.1667\text{ m/s}) \times (7850\text{ kg/m}^3) = 1.480 \times 10^{-3}\text{ kg/s} m ˙ = A ⋅ v w ⋅ ρ m = ( 1.131 × 1 0 − 6 m 2 ) × ( 0.1667 m/s ) × ( 7850 kg/m 3 ) = 1.480 × 1 0 − 3 kg/s
Using the thermal energy balance P ext = m ˙ c p Δ T P_{\text{ext}} = \dot{m} c_p \Delta T P ext = m ˙ c p Δ T : Δ T = P ext m ˙ ⋅ c p = 1357.8 W ( 1.480 × 10 − 3 kg/s ) ( 620 J/kg ⋅ ∘ C ) = 1357.8 0.9176 = 1479.7 ∘ C \Delta T = \frac{P_{\text{ext}}}{\dot{m} \cdot c_p} = \frac{1357.8\text{ W}}{(1.480 \times 10^{-3}\text{ kg/s})(620\text{ J/kg}\cdot^\circ\text{C})} = \frac{1357.8}{0.9176} = 1479.7^\circ\text{C} Δ T = m ˙ ⋅ c p P ext = ( 1.480 × 1 0 − 3 kg/s ) ( 620 J/kg ⋅ ∘ C ) 1357.8 W = 0.9176 1357.8 = 1479. 7 ∘ C
Engineering Insight: The calculated Δ T ≈ 1480 ∘ C \Delta T \approx 1480^\circ\text{C} Δ T ≈ 148 0 ∘ C indicates that Joule heating alone brings the steel wire almost directly to its solidus/liquidus melting temperature ( 1450 ∘ C − 1520 ∘ C 1450^\circ\text{C}-1520^\circ\text{C} 145 0 ∘ C − 152 0 ∘ C ) before it even enters the arc! This illustrates why electrode extension is such a potent variable in continuous wire processes: modest changes in stickout alter the balance between resistance preheating and arc column melting.
- 6. Real-World Engineering Scenarios & Exam Pitfalls
- Practical Industrial Scenario
On a shipyard fabrication berth, welders using flux-cored arc welding (FCAW) experienced intermittent porosity, cold lap, and poor penetration. Welding procedure specifications (WPS) required 28 V 28\text{ V} 28 V and 280 A 280\text{ A} 280 A . The welding power source display in the substation indicated 28.5 V 28.5\text{ V} 28.5 V . However, the leads were 60 m 60\text{ m} 60 m long ( 120 m 120\text{ m} 120 m total loop) of 1/0 AWG cable ( R = 0.39 m Ω / m R = 0.39\text{ m}\Omega/\text{m} R = 0.39 m Ω/ m , total R = 0.0468 Ω R = 0.0468\ \Omega R = 0.0468 Ω ), coiled in tight loops on steel staging.
Diagnostic Investigation: The resistance of the coiled, overheated leads plus worn magnetic ground clamps totaled R loop = 0.065 Ω R_{\text{loop}} = 0.065\ \Omega R loop = 0.065 Ω . At 280 A 280\text{ A} 280 A , the voltage drop across the cables was: V drop = 280 A × 0.065 Ω = 18.2 V V_{\text{drop}} = 280\text{ A} \times 0.065\ \Omega = 18.2\text{ V} V drop = 280 A × 0.065 Ω = 18.2 V
The actual voltage at the welding arc was only 28.5 V − 18.2 V = 10.3 V 28.5\text{ V} - 18.2\text{ V} = 10.3\text{ V} 28.5 V − 18.2 V = 10.3 V . The welders were attempting to operate in short-circuit mode under parameters qualified for globular/spray transfer. Installing 4/0 AWG uncoiled leads and replacing worn spring clamps restored arc voltage to 26.8 V 26.8\text{ V} 26.8 V , eliminating all lack-of-fusion defects.
Common CWEng Exam Traps
Exam Trap 1: Polarity & Penetration Reversal Between Processes A major exam trap asks which polarity produces deepest penetration. For GTAW , the correct answer is DCEN (straight polarity, workpiece is anode). For GMAW , the correct answer is DCEP (reverse polarity). Candidates who memorize "DCEN always penetrates deepest" will get consumable electrode questions wrong.
Exam Trap 2: Faceplate Voltage vs Arc Voltage Examination problems frequently supply a voltage reading measured at the power supply terminals and ask for heat input. If cable length and resistance are given, you must subtract the I R I R I R cable and contact drops before calculating true heat input. Using power source terminal voltage will dramatically overestimate heat input.
Exam Trap 3: Treating the Arc Column as an Ohmic Resistor Never apply Ohm's Law ( V = I R V = IR V = I R ) to solve for arc column behavior under changing current. The arc is an ionized gas whose resistance drops as current rises due to increased ionization density. Doubling current does NOT double arc voltage; arc voltage remains relatively constant or changes only slightly.