7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization
Key Takeaways Explain This Topic AI
The total electrical potential across a welding arc comprises three discrete series zones: the microscopic cathode fall (Vc, 5-15 V), the quasi-neutral plasma column (Vp = Ep * L_arc, 1-2.5 V/mm), and the anode fall (Va, 1-5 V).
Refractory cathodes (tungsten) sustain thermionic emission governed by the Richardson-Dushman equation, where oxide dopants (ThO2, La2O3, CeO2) lower the work function from 4.55 eV to ~2.6 eV, dramatically reducing tip operating temperature and preventing tungsten erosion.
Non-refractory metals (steel, aluminum) cannot reach thermionic emission temperatures without boiling; their arcs rely on high-velocity, mobile non-thermionic cathode spots operating via Fowler-Nordheim field emission (current densities 10^6 to 10^8 A/cm^2).
Metal vapors (Fe: 7.9 eV, Mn: 7.4 eV, Al: 6.0 eV, K: 4.3 eV) possess ionization potentials far below argon (15.76 eV) and helium (24.59 eV); even 1% metal vapor in the arc column supplies the majority of free electrons, governing plasma electrical conductivity.
Last updated: September 2026
7.2 Arc Physics, Ionization Potentials, Work Functions & Plasma Column Mechanics
Quick Answer: A welding arc is a sustained electrical discharge through a high-temperature, quasi-neutral ionized gas known as a thermal plasma . The total arc voltage is non-uniformly distributed across three distinct regions: the cathode fall ( V c ≈ 5 to 15 V V_c \approx 5\text{ to }15\text{ V} V c ≈ 5 to 15 V ), the plasma column ( V p = E p ⋅ L arc V_p = E_p \cdot L_{\text{arc}} V p = E p ⋅ L arc ), and the anode fall ( V a ≈ 1 to 5 V V_a \approx 1\text{ to }5\text{ V} V a ≈ 1 to 5 V ). Cathode electron generation occurs via thermionic emission on refractory tungsten electrodes (enhanced by low-work-function oxide dopants like La 2 O 3 \text{La}_2\text{O}_3 La 2 O 3 and ThO 2 \text{ThO}_2 ThO 2 ) or via mobile, high-density non-thermionic cathode spots (field emission) on consumable steel and aluminum wires. Shielding gas ionization potentials ( 15.76 eV 15.76\text{ eV} 15.76 eV for Ar, 24.59 eV 24.59\text{ eV} 24.59 eV for He) determine arc striking difficulty and thermal conductivity, but volatilized metal vapors ( 4.3 to 7.9 eV 4.3\text{ to }7.9\text{ eV} 4.3 to 7.9 eV ) dominate central column electrical conductivity. Furthermore, geometric arc constriction at the electrode tip induces a radial Lorentz magnetic pinch force ( J × B \mathbf{J} \times \mathbf{B} J × B ) that drives a high-speed axial Maecker plasma jet ( 100 to 500 m/s 100\text{ to }500\text{ m/s} 100 to 500 m/s ) toward the workpiece, governing weld penetration profiles.
1. Structure of the Electric Arc: Voltage Distribution & Fall Regions
A welding arc is not an Ohmic resistor; it is a gaseous electrical conductor characterized by intense thermal and electrical boundary layers adjacent to each metallic electrode. Electrical Potential (V)
- ^
- | +--- Plasma Column (V_p = E_p * L_arc) ---+
- | / /
- V_total +------------+ +---
- | | | |
- | Cathode | | Anode
- | Fall (V_c) | | Fall (V_a)
- | [5-15 V] | | [1-5 V]
- | ~10^-4 cm | | ~10^-3 cm
- 0 +---+----------+---------------------------------------------+---+----> Axial Distance (z)
- Cathode Anode
- (Tungsten) (Workpiece)
The total potential drop across the arc ( V arc V_{\text{arc}} V arc ) is the sum of three discrete components in series: V arc = V c + V p + V a V_{\text{arc}} = V_c + V_p + V_a V arc = V c + V p + V a
1. The Cathode Fall Region ( V c V_c V c )
Spatial Extent: Confined to a microscopic sheath of thickness approximately equal to the electron mean free path ( 10 − 5 to 10 − 4 cm 10^{-5}\text{ to }10^{-4}\text{ cm} 1 0 − 5 to 1 0 − 4 cm , or 0.1 to 1.0 μ m 0.1\text{ to }1.0\ \mu\text{m} 0.1 to 1.0 μ m ).
Physics: Because electrons are light and accelerate away instantly while heavy positive gas ions move slowly, a dense positive space-charge sheath accumulates adjacent to the cathode surface.
Electric Field: The potential drop ( V c ≈ 5 to 15 V V_c \approx 5\text{ to }15\text{ V} V c ≈ 5 to 15 V ) across this sub-micron gap establishes an immense localized electric field: E c = V c d c ≈ 10 V 10 − 5 cm = 10 6 V/cm E_c = \frac{V_c}{d_c} \approx \frac{10\text{ V}}{10^{-5}\text{ cm}} = 10^6\text{ V/cm} E c = d c V c ≈ 1 0 − 5 cm 10 V = 1 0 6 V/cm This colossal field extracts electrons from the metal lattice and accelerates positive ions downward to bombard the cathode surface, maintaining cathode temperature.
2. The Plasma Column ( V p V_p V p )
Spatial Extent: Spans the physical gap between the cathode and anode sheaths ( L arc ≈ 2 to 10 mm L_{\text{arc}} \approx 2\text{ to }10\text{ mm} L arc ≈ 2 to 10 mm ).
Physics: A quasi-neutral, thermally ionized gaseous conductor containing equal densities of positive ions and free electrons ( n e ≈ n i ≈ 10 16 to 10 18 cm − 3 n_e \approx n_i \approx 10^{16}\text{ to }10^{18}\text{ cm}^{-3} n e ≈ n i ≈ 1 0 16 to 1 0 18 cm − 3 ). The plasma is in Local Thermodynamic Equilibrium (LTE) , meaning electron temperature ( T e T_e T e ) and heavy particle gas temperature ( T g T_g T g ) are virtually identical ( T e ≈ T g ≈ 10 , 000 to 25 , 000 K T_e \approx T_g \approx 10,000\text{ to }25,000\text{ K} T e ≈ T g ≈ 10 , 000 to 25 , 000 K ).
Electric Field: The column voltage is proportional to arc length: V p = E p ⋅ L arc V_p = E_p \cdot L_{\text{arc}} V p = E p ⋅ L arc where E p E_p E p is the column electric field gradient ( 1.0 to 1.5 V/mm 1.0\text{ to }1.5\text{ V/mm} 1.0 to 1.5 V/mm in pure Argon; 2.5 to 4.0 V/mm 2.5\text{ to }4.0\text{ V/mm} 2.5 to 4.0 V/mm in pure Helium).
3. The Anode Fall Region ( V a V_a V a )
Spatial Extent: Boundary sheath adjacent to the positive electrode ( 10 − 4 to 10 − 3 cm 10^{-4}\text{ to }10^{-3}\text{ cm} 1 0 − 4 to 1 0 − 3 cm ).
Physics: Under high current, electrons streaming toward the anode create a negative space-charge layer, producing a small anode fall voltage ( V a ≈ 1 to 5 V V_a \approx 1\text{ to }5\text{ V} V a ≈ 1 to 5 V ). The anode fall accelerates incoming electrons directly into the anode surface, releasing their kinetic energy.
2. Cathode Emission Mechanisms & Material Work Functions
Electrons do not freely leave a metal; they must overcome an energy barrier known as the work function ( Φ \Phi Φ ), which is the minimum energy required to remove an electron from the Fermi energy level of the solid conductor to infinity in a vacuum. Thermionic Emission (Refractory Cathode) Non-Thermionic Emission (Cold Cathode)
Example: Pure or Doped Tungsten (GTAW) Example: Carbon Steel / Aluminum (GMAW)
- Electrons Boiled Off Thermally Electrons Extracted by Intense Field
- Over Entire Tip Area (10^3 A/cm^2) at Mobile Micro-Spots (10^6 - 10^8 A/cm^2)
- /// e- /// e- e- e-
- /// e- /// ^ ^ ^
- +----------+ | | |
- | Tungsten | +----+ +----+ +----+
- | Cathode | |Spot| |Spot| |Spot|
- | (>3500K)| +----+---+----+---+----+
- +----------+ | Base Metal Plate |
- +-----------------------+
- Thermionic Emission (Refractory Metals)
Refractory metals like Tungsten ( W W W , melting point 3422 ∘ C 3422^\circ\text{C} 342 2 ∘ C , boiling point 5555 ∘ C 5555^\circ\text{C} 555 5 ∘ C ) can be heated to temperatures above 3000 K 3000\text{ K} 3000 K without melting or excessively boiling away. At these temperatures, thermal kinetic energy enables electrons to overcome the surface work function.
The thermionic current density ( J th J_{\text{th}} J th ) is governed by the classical Richardson-Dushman equation : J th = A R ⋅ T 2 ⋅ exp ( − e Φ k B T ) J_{\text{th}} = A_R \cdot T^2 \cdot \exp\left(-\frac{e\Phi}{k_B T}\right) J th = A R ⋅ T 2 ⋅ exp ( − k B T e Φ )
where A R = 4 π m e k B 2 e ℏ 3 ≈ 1.20 × 10 6 A/(m 2 ⋅ K 2 ) A_R = \frac{4\pi m_e k_B^2}{e \hbar^3} \approx 1.20 \times 10^6\text{ A/(m}^2\cdot\text{K}^2) A R = e ℏ 3 4 π m e k B 2 ≈ 1.20 × 1 0 6 A/(m 2 ⋅ K 2 ) is Richardson's constant, T T T is absolute temperature, k B k_B k B is Boltzmann's constant, and e Φ e\Phi e Φ is the material work function in Joules.
Because of the exponential dependence on − Φ / T -\Phi/T − Φ/ T , lowering the work function drastically increases electron emission at a given temperature , or allows the cathode to operate at a vastly lower temperature for the same current density.
Electrode Material AWS Classification Work Function ( Φ \Phi Φ ) Max Operating Temp Arc Starting & Tip Retention
Pure Tungsten EWP (Green) 4.55 eV 4.55\text{ eV} 4.55 eV ∼ 3800 K \sim 3800\text{ K} ∼ 3800 K Poor starting; rapid tip balling; prone to spitting on DCEN.
Thoriated Tungsten ( 2 % ThO 2 2\%\text{ ThO}_2 2% ThO 2 ) EWTh-2 (Red) 2.63 eV 2.63\text{ eV} 2.63 eV ∼ 3000 K \sim 3000\text{ K} ∼ 3000 K Excellent starting; maintains sharp ground point; low radio-toxicity concern.
Lanthanated Tungsten ( 2 % La 2 O 3 2\%\text{ La}_2\text{O}_3 2% La 2 O 3 ) EWLa-2 (Blue) 2.70 eV 2.70\text{ eV} 2.70 eV ∼ 3100 K \sim 3100\text{ K} ∼ 3100 K Superior non-radioactive replacement; universal AC/DC performance.
Ceriated Tungsten ( 2 % CeO 2 2\%\text{ CeO}_2 2% CeO 2 ) EWCe-2 (Grey) 2.60 eV 2.60\text{ eV} 2.60 eV ∼ 2900 K \sim 2900\text{ K} ∼ 2900 K Outstanding low-amperage starting; ideal for precision orbital tube welding.
Non-Thermionic Emission (Cold Cathodes / Field Emission)
Non-refractory metals (Iron: T b = 2862 ∘ C T_b = 2862^\circ\text{C} T b = 286 2 ∘ C , Aluminum: T b = 2470 ∘ C T_b = 2470^\circ\text{C} T b = 247 0 ∘ C , Copper: T b = 2562 ∘ C T_b = 2562^\circ\text{C} T b = 256 2 ∘ C ) boil violently far below the temperatures needed for thermionic emission. When operated as cathodes (e.g., GMAW DCEN, or GTAW DCEP cleaning half-cycle on aluminum):
Mechanism: Electron emission is driven by Field Emission (Fowler-Nordheim mechanics) and localized micro-explosions.
Cathode Spots: Emission is concentrated into microscopic, highly mobile points called cathode spots ( d spot ≈ 1 to 10 μ m d_{\text{spot}} \approx 1\text{ to }10\ \mu\text{m} d spot ≈ 1 to 10 μ m ). The local current density reaches staggering levels: J spot ≈ 10 6 to 10 8 A/cm 2 J_{\text{spot}} \approx 10^6\text{ to }10^8\text{ A/cm}^2 J spot ≈ 1 0 6 to 1 0 8 A/cm 2
Oxide Sputtering (Cathodic Etching): In aluminum welding under DCEP, cathode spots actively seek out and explode refractory surface oxides ( Al 2 O 3 \text{Al}_2\text{O}_3 Al 2 O 3 , melting point 2072 ∘ C 2072^\circ\text{C} 207 2 ∘ C vs base Al at 660 ∘ C 660^\circ\text{C} 66 0 ∘ C ) because the oxide films possess lower work functions and microscopic surface asperities that concentrate the electrostatic field, stripping the oxide and leaving clean metallic substrate for fusion.
Anode Energy Transfer Physics
Electrons crossing the anode sheath deliver thermal energy via three distinct thermodynamic mechanisms: Q anode = I ( V a + Φ a + 5 2 k B T e e ) Q_{\text{anode}} = I \left( V_a + \Phi_a + \frac{5}{2} \frac{k_B T_e}{e} \right) Q anode = I ( V a + Φ a + 2 5 e k B T e )
where:
I ⋅ V a I \cdot V_a I ⋅ V a is the kinetic energy acquired falling through the anode voltage drop.
I ⋅ Φ a I \cdot \Phi_a I ⋅ Φ a is the electronic condensation heat (the energy released when free electrons condense into the metal conduction band, releasing the anode work function).
I ⋅ ( 5 2 k B T e e ) I \cdot \left(\frac{5}{2} \frac{k_B T_e}{e}\right) I ⋅ ( 2 5 e k B T e ) is the thermal enthalpy carried by the electron gas exiting the high-temperature plasma column ( T e ≈ 10 , 000 to 15 , 000 K T_e \approx 10,000\text{ to }15,000\text{ K} T e ≈ 10 , 000 to 15 , 000 K ).
CWEng Distinction: The electron condensation term ( I ⋅ Φ a I \cdot \Phi_a I ⋅ Φ a ) is why the anode receives such concentrated heat input in arc welding. On a steel workpiece ( Φ a ≈ 4.5 V \Phi_a \approx 4.5\text{ V} Φ a ≈ 4.5 V equivalent), condensing electrons release 4.5 Watts per Ampere 4.5\text{ Watts per Ampere} 4.5 Watts per Ampere directly into the puddle, explaining why DCEN GTAW concentrates 70 % 70\% 70% of its heat into the workpiece anode.
3. Shielding Gas vs Metal Vapor Ionization Thermodynamics
For a gas to conduct electric current, neutral atoms must be stripped of orbital electrons to produce free electron-ion pairs. The degree of thermal ionization is governed by the Saha equation : n e ⋅ n i n n = 2 g i g n ( 2 π m e k B T h 2 ) 3 / 2 exp ( − e V i k B T ) \frac{n_e \cdot n_i}{n_n} = \frac{2 g_i}{g_n} \left( \frac{2\pi m_e k_B T}{h^2} \right)^{3/2} \exp\left(-\frac{e V_i}{k_B T}\right) n n n e ⋅ n i = g n 2 g i ( h 2 2 π m e k B T ) 3/2 exp ( − k B T e V i )
where n e , n i , n n n_e, n_i, n_n n e , n i , n n are the number densities of electrons, ions, and neutral atoms, and V i V_i V i is the first ionization potential of the element. Ionization Energy (eV)
- 25 + 24.59 eV (Helium) <-- Extremely Difficult to Ionize, High Arc Voltage
- |
- 20 +
- | 15.76 eV (Argon) <-- Standard Inert Shielding, Easy Starting
- 15 + 14.40 eV (CO2 effective)
- |
- 10 +
- | 7.90 eV (Iron) <-- Metal Vapors Ionize at Low Temperatures
- 5 + 7.43 eV (Manganese)
- | 4.34 eV (Potassium) <-- Arc Stabilizers in SMAW / FCAW Flux Coatings
- 0 +--------------------------------------------------------------------> Elements
- Ionization Potentials of Shielding Gases and Elements
Element / Molecule Chemical Symbol First Ionization Potential ( V i V_i V i ) Thermal Conductivity Peak Arc Column Behavioral Characteristics
Helium He \text{He} He 24.59 eV 24.59\text{ eV} 24.59 eV Very High ( > 15 , 000 K >15,000\text{ K} > 15 , 000 K ) Highest arc voltage ( 2.5 − 4 V/mm 2.5-4\text{ V/mm} 2.5 − 4 V/mm ); broad, parabolic penetration; difficult HF arc start; exceptional heat transfer for thick Cu/Al.
Argon Ar \text{Ar} Ar 15.76 eV 15.76\text{ eV} 15.76 eV Moderate ( 10 , 000 K 10,000\text{ K} 10 , 000 K ) Easy arc starting; low arc voltage ( 1.0 − 1.5 V/mm 1.0-1.5\text{ V/mm} 1.0 − 1.5 V/mm ); finger-like axial spray penetration; stable quiet arc.
Carbon Dioxide CO 2 \text{CO}_2 CO 2 ∼ 14.0 eV \sim 14.0\text{ eV} ∼ 14.0 eV High at 2000 − 3000 K 2000-3000\text{ K} 2000 − 3000 K (dissociation) Dissociates ( CO 2 ⟷ CO + O \text{CO}_2 \longleftrightarrow \text{CO} + \text{O} CO 2 ⟷ CO + O ); severe thermal constriction; high voltage; repulsive globular transfer.
Iron Vapor Fe \text{Fe} Fe 7.90 eV 7.90\text{ eV} 7.90 eV Low Ionizes at half the energy of Ar; supplies free electrons to core; reduces central plasma temperature.
Manganese Vapor Mn \text{Mn} Mn 7.43 eV 7.43\text{ eV} 7.43 eV Low Highly volatile alloy addition; readily ionizes in GMAW/FCAW arcs.
Aluminum Vapor Al \text{Al} Al 5.99 eV 5.99\text{ eV} 5.99 eV Low Highly mobile vapor sheath; forms diffuse arc column in GMAW-Al.
Potassium K \text{K} K 4.34 eV 4.34\text{ eV} 4.34 eV N/A Arc stabilizer in E6010, E7018 flux coatings; emits abundant electrons to sustain AC zero-crossings.
Sodium Na \text{Na} Na 5.14 eV 5.14\text{ eV} 5.14 eV N/A Arc stabilizer and slag former in EXX15/EXX18 basic electrode coatings.
The Metal Vapor Effect on Arc Plasma Conductivity
In consumable electrode processes (GMAW, FCAW, SMAW), the liquid wire tip boils, introducing metallic vapor into the plasma core. Because the ionization potential of iron ( 7.90 eV 7.90\text{ eV} 7.90 eV ) is roughly half that of argon ( 15.76 eV 15.76\text{ eV} 15.76 eV ), the Boltzmann factor exp ( − e V i / k B T ) \exp(-e V_i / k_B T) exp ( − e V i / k B T ) is orders of magnitude larger for iron at 8000 to 12 , 000 K 8000\text{ to }12,000\text{ K} 8000 to 12 , 000 K .
As a consequence, even a tiny fraction ( 1 % to 2 % 1\%\text{ to }2\% 1% to 2% ) of metallic vapor in the arc column supplies more than 90 % 90\% 90% of all free conduction electrons . This causes:
A reduction in the central core temperature (from ∼ 18 , 000 K \sim 18,000\text{ K} ∼ 18 , 000 K down to ∼ 11 , 000 K \sim 11,000\text{ K} ∼ 11 , 000 K ) because fewer high-energy thermal collisions are needed to liberate charge carriers.
An expansion of the electrically conductive channel width.
Lower overall arc column resistance.