8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing
Key Takeaways Explain This Topic AI
GTAW operates with a non-consumable tungsten electrode whose electron emission, arc stability, and resistance to thermal degradation are determined by the thermionic work function (φ); rare-earth oxide additions (ThO2, CeO2, La2O3) lower φ, reduce operating temperatures, and prevent tungsten spitting.
Tungsten electrode geometry—specifically vertex angle (included grind angle) and truncation flat diameter—controls current density, magnetic pinch forces, arc pressure (P_arc ∝ I²), and weld pool aspect ratios (sharp angles <30° produce wide shallow beads; blunt angles 60°–90° create deep narrow penetration).
Shielding gas selection dictates arc voltage and thermal enthalpy: Argon facilitates low-energy arc starting and cathode cleaning on AC; Helium elevates arc voltage by 50–100% and transfers intense heat for thick sections; Ar-H2 mixtures accelerate travel speed on austenitic stainless steel but cause cracking in ferritic steels.
Plasma Arc Welding (PAW) constricts the arc column through a water-cooled copper orifice nozzle, boosting arc temperatures to 20,000–30,000 K and increasing energy density to >10⁵ W/cm² to create a columnar, low-divergence plasma jet.
In PAW keyhole mode, plasma stagnation pressure and gas momentum pierce through plate thicknesses up to 12 mm in a single pass without edge beveling, balancing hydrostatic liquid head and surface tension forces to form a full-penetration keyhole.
Last updated: September 2026
8.3 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing
Quick Answer: Gas Tungsten Arc Welding (GTAW) and Plasma Arc Welding (PAW) utilize non-consumable tungsten electrodes to generate highly stable, slag-free electric arcs. In GTAW, arc morphology is governed by electrode tip geometry (vertex angle and flat diameter) and thermionic emission: sharp grind angles ( < 30 ∘ <30^\circ < 3 0 ∘ ) disperse the arc plasma, yielding shallow, wide beads, whereas blunt angles ( 60 ∘ – 90 ∘ 60^\circ–90^\circ 6 0 ∘ –9 0 ∘ ) concentrate current density and electromagnetic Lorentz pinch forces, producing deep narrow penetration. Rare-earth oxide additions (ceria, lanthana, thoria) lower the electron work function ( ϕ \phi ϕ ), enhancing arc re-ignition and tip life. PAW advances arc physics by constricting the plasma column through a water-cooled copper orifice nozzle; this constriction elevates plasma velocity and temperature ( > 25 , 000 K >25,000\text{ K} > 25 , 000 K ), enabling "keyhole mode" single-pass full-penetration welds on plates up to 12 mm 12\text{ mm} 12 mm thick without joint beveling.
GTAW Process Physics & Thermionic Electron Emission
In GTAW, the electric arc is sustained between a non-consumable tungsten electrode and the workpiece inside an inert gas blanket. The electrode functions as a thermionic cathode under Direct Current Electrode Negative (DCEN, straight polarity): (-) DCEN Power Supply
- |
- V
- +-------------------+
- | Tungsten Electrode|
- +---------+---------+
- / \
- / \ Vertex Angle (θ)
- / | \
- +---+---+
- |d_flat |
- ( | ) Arc Flame
- ( ( ) ) High Current Density Core
- =======================[ M-Pool ]======================= (+) Anode Workpiece
- The Richardson-Dushman Thermionic Emission Equation
The current density of electrons emitted from the heated tungsten cathode tip ( J e J_e J e ) is governed by the Richardson-Dushman relationship: J e = A R T 2 exp ( − ϕ k B T ) J_e = A_R T^2 \exp\left(-\frac{\phi}{k_B T}\right) J e = A R T 2 exp ( − k B T ϕ )
where:
A R A_R A R is Richardson's constant (theoretically 1.20 × 10 6 A / ( m 2 ⋅ K 2 ) 1.20 \times 10^6\text{ A}/(\text{m}^2\cdot\text{K}^2) 1.20 × 1 0 6 A / ( m 2 ⋅ K 2 ) ),
- T T T is absolute surface temperature of the cathode (K),
- ϕ \phi ϕ is the electronic work function of the electrode surface ( eV \text{eV} eV ),
k B k_B k B is the Boltzmann constant ( 8.617 × 10 − 5 eV/K 8.617 \times 10^{-5}\text{ eV/K} 8.617 × 1 0 − 5 eV/K ).
Because electron emission varies exponentially with − ϕ / k B T -\phi/k_B T − ϕ / k B T , lowering the work function ( ϕ \phi ϕ ) dramatically increases electron current density at a given temperature, or allows the electrode to operate at a significantly cooler temperature for the same current. This minimizes tungsten erosion, eliminates spitting, and stabilizes the cathode spot.
Tungsten Electrode Classifications & Metallurgy (AWS A5.12 / ISO 6848)
Tungsten has the highest melting point of all metals ( 3422 ∘ C 3422^\circ\text{C} 342 2 ∘ C / 6192 ∘ F 6192^\circ\text{F} 619 2 ∘ F ). To optimize thermionic performance, manufacturers dope pure tungsten with 1 % – 2 % 1\%–2\% 1%–2% of stable rare-earth metal oxides.
AWS A5.12 Tungsten Electrode Specifications
AWS Classification Color Band Oxide Addition Work Function ( ϕ \phi ϕ ) Operating Polarity Industrial Applications & Characteristics
EWP Green None ( 99.5 % W 99.5\%\text{ W} 99.5% W ) 4.50 eV 4.50\text{ eV} 4.50 eV AC only Forms clean rounded/balled tip on AC; used for non-critical Al/Mg; poor DC ignition.
EWTh-2 Red 1.7 – 2.2 % ThO 2 1.7–2.2\%\ \text{ThO}_2 1.7–2.2% ThO 2 (Thoria) 2.60 eV 2.60\text{ eV} 2.60 eV DCEN Low work function; superior tip longevity; low radioactivity (requires dedicated dust extraction during grinding).
EWCe-2 Orange 1.8 – 2.2 % CeO 2 1.8–2.2\%\ \text{CeO}_2 1.8–2.2% CeO 2 (Ceria) 2.70 eV 2.70\text{ eV} 2.70 eV DCEN or AC Non-radioactive direct replacement for thoriated; excellent low-current arc starts (orbital tube welding).
EWLa-1.5 Gold 1.3 – 1.7 % La 2 O 3 1.3–1.7\%\ \text{La}_2\text{O}_3 1.3–1.7% La 2 O 3 (Lanthana) 2.65 eV 2.65\text{ eV} 2.65 eV DCEN or AC Universal premium choice; resist thermal thermal shock; lowest erosion rate at high currents.
EWLa-2 Blue 1.8 – 2.2 % La 2 O 3 1.8–2.2\%\ \text{La}_2\text{O}_3 1.8–2.2% La 2 O 3 (Lanthana) 2.60 eV 2.60\text{ eV} 2.60 eV DCEN or AC Exceptional ignition stability; extended tip longevity across heavy automated manufacturing.
EWZr-1 Brown 0.15 – 0.40 % ZrO 2 0.15–0.40\%\ \text{ZrO}_2 0.15–0.40% ZrO 2 (Zirconia) 3.50 eV 3.50\text{ eV} 3.50 eV AC only Resists tungsten contamination in radiographic-quality aluminum aerospace welding.
Electrode Tip Geometry and Arc Pressure Mechanics
The preparation of the tungsten tip dictates current density distribution, magnetic arc constriction, and weld puddle geometry. SHARP TIP (θ = 15° - 30°) BLUNT TIP (θ = 60° - 90° with Flat)
- | |
- / \ Small Arc Flame | |
- / \ (Dispersed Jet) / \ Intense Lorentz Pinch
- / . \ / _ \ Constricted Plasma Core
- +----+----+ +---+-----+ (Deep Digging Force)
- ( ) | |
- ( ) Broad, Shallow Arc ( )
- ===[ Puddle ]=== ====[ | ]==== Narrow, Deep Penetration
- Vertex Angle ( θ \theta θ ) and Truncation Flat ( d flat d_{\text{flat}} d flat )
Sharp Vertex Angle ( θ < 30 ∘ \theta < 30^\circ θ < 3 0 ∘ ):
Spreads the cathode attachment area over a longer conical surface.
Produces a divergent, wide arc cone with lower current density.
Results in a shallow, wide weld bead profile.
Prone to tip overheating, erosion, and tungsten inclusion at high current.
Blunt Vertex Angle ( θ = 60 ∘ – 90 ∘ \theta = 60^\circ–90^\circ θ = 6 0 ∘ –9 0 ∘ with a Truncated Flat):
Forces the cathode emission spot to attach to the tiny flat end ( d flat ≈ 0.25 – 0.8 mm d_{\text{flat}} \approx 0.25–0.8\text{ mm} d flat ≈ 0.25–0.8 mm ).
Greatly intensifies the self-induced magnetic pinch force: P arc ≈ μ 0 I 2 4 π r spot 2 P_{\text{arc}} \approx \frac{\mu_0 I^2}{4 \pi r_{\text{spot}}^2} P arc ≈ 4 π r spot 2 μ 0 I 2
Generates a stiff, high-velocity plasma jet directed downward into the pool.
Produces deep, narrow joint penetration with a high depth-to-width aspect ratio, reducing angular joint distortion.
Grinding Direction:
Grinding marks must run longitudinally (parallel to the electrode axis). Transverse grinding creates circumferential ridges that force the arc to jump erratically between peaks, causing arc wander, high-frequency instability, and premature tungsten disintegration.
- Shielding Gases & Arc Initiation Systems
- Shielding Gas Physics in GTAW
Pure Argon (Ar): Benchmark gas. Low thermal conductivity and low ionization potential provide effortless arc starting, smooth cathode cleaning on AC, and stable arc operation. Concentrates heat in the center line.
Helium and Ar-He Mixtures ( 25 – 75 % He 25–75\%\text{ He} 25–75% He ): Helium has twice the thermal conductivity of Argon and a higher ionization potential ( 24.6 eV 24.6\text{ eV} 24.6 eV ). At equivalent arc lengths, pure Helium increases arc voltage by 60 – 100 % 60–100\% 60–100% , tripling total heat input. Essential for thick aluminum, high-conductivity copper, and high-speed tube mills.
Argon-Hydrogen Mixtures ( 95 % Ar / 5 % H 2 95\%\text{ Ar} / 5\%\text{ H}_2 95% Ar /5% H 2 ): Hydrogen dissociates in the arc and releases intense heat upon recombining at the plate. Adding 2 – 5 % H 2 2–5\%\text{ H}_2 2–5% H 2 increases travel speeds by 50 % 50\% 50% and produces exceptionally clean, oxide-free beads on 300-series austenitic stainless steels and nickel alloys. Strict Warning: Hydrogen additions cause catastrophic cold cracking in carbon, low-alloy, and martensitic steels, and porosity in aluminum and copper.
- Arc Initiation Systems 1. HIGH-FREQUENCY (HF) SPARK 2. LIFT-ARC (MICRO-CURRENT)
- No Physical Contact Physical Touch -> Controlled Lift
- Tungsten Tip Tungsten Tip
- | |
- - -|- - - (Ionized HF Spark) V Touches Plate (Low Current: ~10A)
- ============ Base Metal =====+===== (Retracts -> Full Current Arc)
High-Frequency (HF) Start: A high-voltage ( 3000 – 5000 V 3000–5000\text{ V} 3000–5000 V ), high-frequency ( > 1 MHz >1\text{ MHz} > 1 MHz ) spark breaks down the dielectric resistance of the shielding gas gap, ionizing the gas and establishing the welding arc without physical contact. Avoids tungsten contamination, but HF radiation causes severe electromagnetic interference (EMI) with nearby CNC controllers and computers.
Lift-Arc Initiation: Microprocessor-controlled touch start. The electrode touches the work with a tiny sensing current ( < 10 A <10\text{ A} < 10 A ). Once contact is detected, the welder lifts the torch; upon lift-off, the machine instantly ignites the main arc. Eliminates tungsten contamination and EMI.
Scratch Start: Striking the electrode like a match. Strictly prohibited on nuclear, aerospace, and high-purity piping because it deposits brittle tungsten inclusions in the joint root.
Plasma Arc Welding (PAW): Orifice Constriction & Modes
Plasma Arc Welding is an advanced extension of GTAW where the arc column is constricted by a water-cooled copper orifice nozzle. GTAW (TIG) PLASMA ARC (PAW)
Unconstricted Arc Constricted Arc
- +---------------+ +---------------+ Electrode
- | Tungsten | | Tungsten | Inside Nozzle
- +-------+-------+ +-------+-------+
- | |
- V V Orifice Gas (Ar)
- [=====|===|=====] Water-Cooled
- / \ | | Copper Orifice
- / \ Constriction -> | P | Collimated Plasma Jet
- ===================[ Puddle ]==================== [=====] Shielding Gas Nozzle
- Divergent Arc Cone (Low Energy Density) ====[Keyhole]==== High Energy Density
- Orifice Physics and Arc Constriction
In standard GTAW, the arc cone is free to diverge, resulting in temperatures of 10 , 000 – 16 , 000 K 10,000–16,000\text{ K} 10 , 000–16 , 000 K and an energy density of approximately 10 4 W/cm 2 10^4\text{ W/cm}^2 1 0 4 W/cm 2 . In PAW, forcing the plasma through a nozzle orifice ( d orifice = 1.0 – 3.5 mm d_{\text{orifice}} = 1.0–3.5\text{ mm} d orifice = 1.0–3.5 mm ) restricts radial expansion. To sustain current conduction through this tiny channel:
The plasma gas undergoes severe thermal ionization.
Column temperature surges to 20 , 000 – 30 , 000 K 20,000–30,000\text{ K} 20 , 000–30 , 000 K .
Plasma gas velocity accelerates to near-sonic speeds.
Energy density exceeds 10 5 – 10 6 W/cm 2 10^5–10^6\text{ W/cm}^2 1 0 5 –1 0 6 W/cm 2 .
The arc emerges as a collimated cylinder, making arc voltage and penetration virtually immune to variations in torch standoff distance.
Transferred vs. Non-Transferred Arc
Transferred Arc: The tungsten electrode is the cathode ( − - − ), and the workpiece is the anode ( + + + ) . The plasma jet extends across the gap to melt the joint. Used for all structural welding, deep keyholing, and cutting.
Non-Transferred Arc: The tungsten electrode is the cathode ( − - − ), and the constricting orifice nozzle itself is the anode ( + + + ) . The arc terminates inside the torch; only the hot exiting plasma flame reaches the work. Used for low-heat brazing, thermal spraying, and non-conductive materials.
PAW Keyhole Mode Mechanics and Force Balance
When plasma gas flow and current exceed threshold values, PAW transitions from traditional "melt-in" mode into keyhole mode . PAW KEYHOLE MECHANICS
- Plasma Jet (High Velocity)
- | |
- V V
- Base Metal +------------+ Base Metal
- ------------------------> | KEYHOLE | <-------------------------
- | Molten Pool | (Vapor | Molten Pool |
- | Flows Around Hole | Cavity) | Flows Around Hole |
- | +------------+ |
- -------------------------------------------------------------------
- | |
- V V Exit Orifice Flame
- The Hydrodynamic Force Balance
In keyhole welding, the stagnation pressure of the plasma jet ( P arc + P plasma P_{\text{arc}} + P_{\text{plasma}} P arc + P plasma ) physically pierces through the entire plate thickness, creating an open vapor cavity. Molten metal is held in equilibrium along the vertical cavity walls by surface tension ( γ \gamma γ ). As the torch moves forward, surface tension forces the liquid metal to flow symmetrically around the keyhole cavity and coalesce at the trailing edge to form a defect-free, full-penetration bead.
The dynamic equilibrium condition to maintain a stable keyhole without blowout is: P arc + P plasma + P vapor = 2 γ r keyhole + ρ g h P_{\text{arc}} + P_{\text{plasma}} + P_{\text{vapor}} = \frac{2\gamma}{r_{\text{keyhole}}} + \rho g h P arc + P plasma + P vapor = r keyhole 2 γ + ρ g h
where:
- r keyhole r_{\text{keyhole}} r keyhole is the radius of the keyhole vapor channel,
- γ \gamma γ is the surface tension of the molten alloy ( N/m \text{N/m} N/m ),
- ρ \rho ρ is the liquid metal density ( kg/m 3 \text{kg/m}^3 kg/m 3 ),
- g g g is gravitational acceleration ( 9.81 m/s 2 9.81\text{ m/s}^2 9.81 m/s 2 ),
h h h is plate thickness (m).
If plasma pressure exceeds surface tension support ( P plasma > 2 γ r + ρ g h P_{\text{plasma}} > \frac{2\gamma}{r} + \rho g h P plasma > r 2 γ + ρ g h ), the keyhole blows out catastrophically, expelling liquid metal and creating an elongated through-hole (blowout defect). If plasma pressure is insufficient, the keyhole collapses, resulting in incomplete penetration.
- Comprehensive Worked Numerical Example: Keyhole Force & Energy Density Modeling
- Problem Statement
A titanium aerospace tank shell ( 6.0 mm 6.0\text{ mm} 6.0 mm thick Grade 2 Titanium) is welded in a single pass using keyhole PAW. The welding parameters are:
- Current I = 185 A I = 185\text{ A} I = 185 A (DCEN)
- Voltage V = 31.0 V V = 31.0\text{ V} V = 31.0 V
- Travel Speed v = 280 mm/min v = 280\text{ mm/min} v = 280 mm/min
- Orifice nozzle diameter d orifice = 2.4 mm d_{\text{orifice}} = 2.4\text{ mm} d orifice = 2.4 mm
- Thermal efficiency η paw = 0.70 \eta_{\text{paw}} = 0.70 η paw = 0.70
- Titanium liquid surface tension γ = 1.65 N/m \gamma = 1.65\text{ N/m} γ = 1.65 N/m
- Liquid density ρ = 4110 kg/m 3 \rho = 4110\text{ kg/m}^3 ρ = 4110 kg/m 3
- Keyhole radius r k = 1.4 mm r_k = 1.4\text{ mm} r k = 1.4 mm
Calculate: (1) the average electrical power density ( q density q_{\text{density}} q density ) entering the constricting orifice, (2) the net heat input per unit length ( H H H ), and (3) the minimum critical internal arc pressure ( P crit P_{\text{crit}} P crit ) required to balance the ferrostatic head and surface tension of the titanium puddle.
Step-by-Step Engineering Solution
Step 1: Calculate Electrical Power Density ( q density q_{\text{density}} q density ) in the Orifice Orifice cross-sectional area: A orifice = π d 2 4 = π ( 2.4 mm ) 2 4 = 4.524 mm 2 = 4.524 × 10 − 2 cm 2 A_{\text{orifice}} = \frac{\pi d^2}{4} = \frac{\pi (2.4\text{ mm})^2}{4} = 4.524\text{ mm}^2 = 4.524 \times 10^{-2}\text{ cm}^2 A orifice = 4 π d 2 = 4 π ( 2.4 mm ) 2 = 4.524 mm 2 = 4.524 × 1 0 − 2 cm 2
Total arc electrical power: P elec = V ⋅ I = 31.0 V ⋅ 185 A = 5735 W P_{\text{elec}} = V \cdot I = 31.0\text{ V} \cdot 185\text{ A} = 5735\text{ W} P elec = V ⋅ I = 31.0 V ⋅ 185 A = 5735 W
Power density entering the constricted nozzle: q density = P elec A orifice = 5735 W 4.524 × 10 − 2 cm 2 = 126 , 768 W/cm 2 ≈ 1.27 × 10 5 W/cm 2 q_{\text{density}} = \frac{P_{\text{elec}}}{A_{\text{orifice}}} = \frac{5735\text{ W}}{4.524 \times 10^{-2}\text{ cm}^2} = 126,768\text{ W/cm}^2 \approx 1.27 \times 10^5\text{ W/cm}^2 q density = A orifice P elec = 4.524 × 1 0 − 2 cm 2 5735 W = 126 , 768 W/cm 2 ≈ 1.27 × 1 0 5 W/cm 2
Observation: This energy density exceeds that of unconstricted GTAW ( 10 4 W/cm 2 ~10^4\text{ W/cm}^2 1 0 4 W/cm 2 ) by an order of magnitude.
Step 2: Calculate Net Heat Input ( H H H ) H = η paw ⋅ V ⋅ I ⋅ 60 1000 ⋅ v = 0.70 ⋅ 31.0 ⋅ 185 ⋅ 60 1000 ⋅ 280 = 240 , 870 280 , 000 = 0.860 kJ/mm H = \frac{\eta_{\text{paw}} \cdot V \cdot I \cdot 60}{1000 \cdot v} = \frac{0.70 \cdot 31.0 \cdot 185 \cdot 60}{1000 \cdot 280} = \frac{240,870}{280,000} = 0.860\text{ kJ/mm} H = 1000 ⋅ v η paw ⋅ V ⋅ I ⋅ 60 = 1000 ⋅ 280 0.70 ⋅ 31.0 ⋅ 185 ⋅ 60 = 280 , 000 240 , 870 = 0.860 kJ/mm
Step 3: Calculate Critical Keyhole Equilibrium Pressure ( P crit P_{\text{crit}} P crit ) The surface tension capillary pressure opposing keyhole collapse is: P cap = 2 γ r k = 2 ⋅ 1.65 N/m 1.4 × 10 − 3 m = 3.30 0.0014 = 2357.1 Pa P_{\text{cap}} = \frac{2\gamma}{r_k} = \frac{2 \cdot 1.65\text{ N/m}}{1.4 \times 10^{-3}\text{ m}} = \frac{3.30}{0.0014} = 2357.1\text{ Pa} P cap = r k 2 γ = 1.4 × 1 0 − 3 m 2 ⋅ 1.65 N/m = 0.0014 3.30 = 2357.1 Pa
The hydrostatic head of the liquid puddle is: P hydro = ρ ⋅ g ⋅ h = ( 4110 kg/m 3 ) ⋅ ( 9.81 m/s 2 ) ⋅ ( 0.006 m ) = 241.9 Pa P_{\text{hydro}} = \rho \cdot g \cdot h = (4110\text{ kg/m}^3) \cdot (9.81\text{ m/s}^2) \cdot (0.006\text{ m}) = 241.9\text{ Pa} P hydro = ρ ⋅ g ⋅ h = ( 4110 kg/m 3 ) ⋅ ( 9.81 m/s 2 ) ⋅ ( 0.006 m ) = 241.9 Pa
Total required balancing pressure: P crit = P cap + P hydro = 2357.1 + 241.9 = 2599.0 Pa ≈ 2.60 kPa P_{\text{crit}} = P_{\text{cap}} + P_{\text{hydro}} = 2357.1 + 241.9 = 2599.0\text{ Pa} \approx 2.60\text{ kPa} P crit = P cap + P hydro = 2357.1 + 241.9 = 2599.0 Pa ≈ 2.60 kPa
- Industrial Scenarios & Certified Welding Engineer Exam Pitfalls
- Real-World Engineering Failure Scenario
An automated manufacturing plant fabricated thin-wall ( 1.5 mm 1.5\text{ mm} 1.5 mm ) 316L stainless steel heat-exchanger tubing using high-speed mechanized GTAW. The line experienced a sudden spike in weld porosity and lack of penetration. Investigation revealed that the shop had switched from ground 2% Ceriated electrodes to Pure Tungsten (EWP, green) to reduce procurement costs, and operators were sharpening electrodes on a standard pedestal grinding wheel with circumferential rotations. The pure tungsten electrodes eroded rapidly under DCEN, developing large balled ends that caused the arc to wander across the seam. Furthermore, circumferential grind marks induced continuous high-frequency arc jumping. The engineer mandated a switch to 1.5% Lanthanated electrodes (EWLa-1.5), installed a dedicated longitudinal diamond grinding fixture with a 50 ∘ 50^\circ 5 0 ∘ vertex angle and 0.5 mm 0.5\text{ mm} 0.5 mm truncation flat, and added 2 % H 2 2\%\text{ H}_2 2% H 2 to the argon shielding gas. The rejection rate dropped to zero.
Common Exam Traps
Exam Trap 1: Using Ar-H2 Shielding Gas on Carbon or Ferritic Steels While Argon-Hydrogen ( 95 % Ar / 5 % H 2 95\%\text{ Ar} / 5\%\text{ H}_2 95% Ar /5% H 2 ) delivers exceptional benefits for austenitic stainless steels (304, 316), applying this gas to carbon steel, HSLA steel, or duplex stainless steel introduces catastrophic amounts of diffusible hydrogen directly into a susceptible martensitic/ferritic lattice, causing immediate Hydrogen-Induced Delayed Cracking (HIC) .
Exam Trap 2: Balled vs. Pointed Tungsten for Polarity A frequent exam misconception is assuming balled tips are used for deep penetration. A rounded/balled tip is strictly formed on Pure or Zirconiated tungsten when welding on AC (Alternating Current) to distribute heat during the DCEP cleaning half-cycle. For all DCEN welding, the electrode tip must be ground to a truncated cone to focus arc current density.
Exam Trap 3: Confusing Orifice Gas and Shielding Gas in PAW Plasma Arc Welding uses two completely separate gas streams: (1) Orifice Gas , which flows through the constricting nozzle around the tungsten to form the high-velocity plasma column (almost exclusively pure Argon at low flow rates, 1 – 5 L/min 1–5\text{ L/min} 1–5 L/min ), and (2) Shielding Gas , which flows from an outer cup to protect the weld puddle from the atmosphere (typically Argon or Ar-He at higher flow rates, 10 – 25 L/min 10–25\text{ L/min} 10–25 L/min ). Swapping or mixing these flow rates will either instantly melt the constricting copper nozzle or blow the weld puddle out of the joint.