Study guide

9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray

AWS CWEng Certified Welding Engineer Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction & CWEng Exam Overview

About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set

2 Chapter 1: Mathematics & Statistics for Welding Engineers

1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers

3 Chapter 2: Physics Fundamentals & Mechanics

2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity

4 Chapter 3: General & Physical Chemistry for Welding

3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection

5 Chapter 4: Strength of Materials & Mechanics of Materials

4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment

6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding

5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments

7 Chapter 6: Electrical Engineering Principles for Welding Systems

6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow

8 Chapter 7: Welding Heat Sources & Arc Physics

7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design

9 Chapter 8: Arc Welding Processes & Parameter Controls

8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems

10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes

9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray

11 Chapter 10: Physical & Transformation Metallurgy of Steels

10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control

12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy

11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences

13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics

12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control

14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis

13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction

15 Chapter 14: Brazing, Soldering & Industrial Welding Safety

14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation

16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation

15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice

17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1

16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation

18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control

17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing

19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics

18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison

9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray

Key Takeaways Explain This Topic AI

High-frequency welding operates in the 200 to 500 kilohertz range, where skin and proximity effects concentrate current on the strip edges to be joined.

Flash welding heats the faying surfaces by arcing and expulsion, then forges them together with an upset stroke that expels oxides and molten metal.

Arc stud welding uses a drawn arc under a ceramic ferrule, while capacitor discharge stud welding discharges stored energy in milliseconds for thin sheet.

Ultrasonic welding joins metals in the solid state using shear oscillation at roughly 20 to 40 kilohertz under clamping force, with no melting.

Weld overlay is metallurgically fused and diluted by the substrate, whereas thermally sprayed coatings bond largely mechanically and are not diluted.

Last updated: September 2026

High-Frequency Welding (HFRW and HFIW)

High-frequency welding is the process behind almost all continuously produced welded tube and pipe. A strip is roll-formed into a tube with an open seam, high-frequency current is introduced either by sliding contacts (HFRW) or by an induction coil (HFIW) , and pressure rolls forge the heated edges together.

Its efficiency comes from two electromagnetic effects:

Skin effect. At high frequency, current crowds into a thin surface layer whose depth falls as frequency rises. Operating in the 200 to 500 kHz range confines current to a few tenths of a millimetre.

Proximity effect. When two conductors carry current in opposite directions, the current concentrates on the facing surfaces. In a tube mill the two strip edges converging on the weld point are exactly such a pair, so the current concentrates precisely where heat is wanted.

The combination heats a very narrow band to forging temperature in milliseconds, and the squeeze rolls expel the softened surface metal with its oxides as flash, which is then trimmed. Line speeds well over 100 metres per minute are routine. The bond is a solid-state forge weld , not a fusion weld, and the classic defect is a cold weld where insufficient heat or upset leaves an unbonded oxide film on the bond line.

Flash Welding (FW) and Upset Welding (UW)

Both are resistance processes that join full cross-sections end to end, and B5.16 lists flash welding among the processes a welding engineer must know.

Flash welding proceeds in three stages:

Flashing. The parts are brought into light contact under current. Localised contact points heat, melt and explode, expelling metal as flashing sparks. Repeated advance sustains the flashing and heats the faying surfaces uniformly.

Upset. The parts are driven together rapidly under high force. Molten metal, oxides and contaminants are expelled radially into the upset flash.

Hold. Force is maintained while the joint cools.

Because the final bond is made between clean, plastically deformed metal after the contaminated layer has been squeezed out, flash welding produces high-integrity joints in rail, chain link, band saw blades, automotive rims and ring forgings. The upset flash is trimmed afterwards.

Upset welding omits the flashing stage: the parts are held in firm contact, resistance heated, and then upset. It suits smaller cross-sections and wire butt joints where surfaces can be prepared clean beforehand.

  • Attribute Flash welding Upset welding
  • Initial contact Light, intermittent Firm, continuous
  • Surface cleaning By expulsion during flashing Requires pre-cleaned surfaces
  • Typical cross-section Large and irregular Small and uniform
  • Material loss Higher (flashing plus upset) Lower
  • Stud Welding

Arc stud welding (SW) places a stud in a gun against the work inside a ceramic ferrule , lifts it to draw an arc, melts both stud end and base metal, then plunges the stud into the pool under spring force. The ferrule contains the molten metal, shields the arc and shapes the fillet. Arc time is a fraction of a second. AWS D1.1 governs stud application qualification and production testing, which is done by bend testing or torque testing rather than by radiography.

Capacitor discharge (CD) stud welding stores energy in a capacitor bank and discharges it through a small ignition tip on the stud end in milliseconds . The extremely short cycle means almost no heat reaches the reverse side, which is why CD studs can be attached to sheet as thin as roughly 0.5 mm without marking the show face. The trade-off is a much smaller weld area and lower load capacity.

Ultrasonic Welding (USW)

Ultrasonic welding is a solid-state process. A sonotrode applies shear oscillation at roughly 20 to 40 kHz to the interface while a clamping force presses the parts together. The oscillation breaks up and disperses surface oxides, brings clean metal into intimate contact, and produces a metallurgical bond by interdiffusion and local plastic flow — without melting .

Its natural applications are thin, highly conductive, oxide-forming metals that resist fusion welding: aluminum and copper foils, battery tabs and busbars, wire harness terminations, and dissimilar aluminum-to-copper joints. Because there is no melt, there is no solidification cracking, no porosity and no brittle fusion-zone intermetallic layer of the kind that plagues fusion welding of aluminum to copper — although a thin intermetallic can still form by diffusion at long weld times.

Surfacing (SW) and Thermal Spraying (THSP)

B5.16 groups surfacing and thermal spraying together, and the distinction between them is a favourite exam discrimination.

Weld Surfacing (Overlay, Cladding, Hardfacing)

Weld surfacing deposits filler metal onto a surface by a fusion welding process to restore dimensions or impart different properties:

Buildup restores worn dimensions with a material similar to the substrate.

Hardfacing applies a wear-resistant deposit such as a chromium carbide or a cobalt-base alloy.

Cladding applies a corrosion-resistant layer such as an austenitic stainless or a nickel alloy.

Buttering deposits a transition layer on one face before making a dissimilar joint.

The defining characteristic is dilution : the deposit melts and mixes with the substrate, so the first layer's chemistry is not the filler's chemistry. Dilution is controlled by process selection, heat input, electrode oscillation and the number of layers, and a corrosion-resistant overlay is normally specified to achieve required chemistry at a stated depth in the second layer.

Thermal Spraying

Thermal spraying melts or softens a consumable and propels the particles onto a prepared substrate, where they flatten and build up a lamellar coating.

  • Variant Heat source Typical use
  • Flame spray (FLSP) Oxyfuel flame Low-cost buildup and corrosion coatings
  • Arc spray (ASP) Twin-wire electric arc Zinc and aluminum anti-corrosion coatings
  • Plasma spray (PSP) Plasma jet Ceramics and high-melting-point coatings
  • High-velocity oxyfuel (HVOF) Supersonic combustion jet Dense, low-porosity carbide wear coatings
  • Cold spray Supersonic gas jet, no melting Oxygen-sensitive metals, dimensional restoration

The critical difference from weld surfacing is the bond. Thermally sprayed coatings adhere primarily by mechanical interlocking to a grit-blasted surface, with little or no fusion and therefore no dilution . The substrate stays cool, so distortion and metallurgical change are minimal — but bond strength is far lower than a fused overlay and the coating is generally not suitable for high-impact service. The exception is spray-and-fuse , where a self-fluxing nickel-chromium-boron-silicon alloy is sprayed and then fused in a subsequent heating operation to create a metallurgical bond.

Exam Trap 1: Calling thermal spray a welding process with dilution. Thermally sprayed coatings bond mechanically and are not diluted by the substrate. If a question asks how to achieve a specified overlay chemistry at the surface, dilution control points to weld overlay; if it asks how to coat without heating the part, it points to thermal spray.

Exam Trap 2: Confusing flash welding with arc welding. Flash welding is a resistance process. The flashing stage expels metal to clean and heat the faying surfaces, and the actual joint is made by the upset forging stroke after the arc-like flashing has stopped.

Exam Trap 3: Assuming ultrasonic welding melts the interface. Ultrasonic welding is solid state. Shear oscillation disrupts oxides and produces bonding by plastic flow and diffusion below the melting point, which is precisely why it works on aluminum and copper.