9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc
AWS CWEng Certified Welding Engineer Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction & CWEng Exam Overview
About the CWEng Exam: Four Parts, 163 Questions & Testing Logistics Scoring, Composite Weighting, Eligibility & Five-Year Renewal How to Use This Guide & Build Your Open-Book Reference Set
2 Chapter 1: Mathematics & Statistics for Welding Engineers
1.1 Engineering Mathematics: Algebra, Trigonometry & Geometry in Weldments 1.2 Differential & Integral Calculus Fundamentals in Engineering Analysis 1.3 Applied Engineering Statistics, Population Distributions & Quality Metrics 1.4 Polynomial Equations, Conic Sections & Complex Numbers
3 Chapter 2: Physics Fundamentals & Mechanics
2.1 Unit Systems, Dimensional Analysis & Engineering Conversions 2.2 Mechanics: Statics, Equilibrium, Force Vectors & Moments 2.3 Work, Energy, Power & Mechanical Advantage in Welding Systems 2.4 Thermal Physics, Linear/Volumetric Expansion & Heat Capacity
4 Chapter 3: General & Physical Chemistry for Welding
3.1 Atomic Structure, Bonding & Solid-Solution Thermodynamics 3.2 Hume-Rothery Compatibility, Interstitial Strain & HSLA Microalloy Scavenging 3.3 Gas Laws, Dalton Partial Pressures, Arc Dissociation & Sieverts Law 3.4 Cylinder Capacity, Available Arc Time & Gas-Related Porosity Diagnosis 3.5 Redox Thermodynamics, Deoxidation & Slag-Metal Refining 3.6 Basicity Index Calculations, Toughness Prediction & Cryogenic Consumable Selection
5 Chapter 4: Strength of Materials & Mechanics of Materials
4.1 Engineering vs. True Stress-Strain, Elastic Constants & Z-Direction Ductility 4.2 Plane Stress vs. Plane Strain, Triaxial Restraint & Alloy Property Comparison 4.3 Beam Bending, Transverse Shear, Torsion & Mohr Circle Construction 4.4 Multiaxial Yield Criteria & Combined-Load Analysis of Welded Members 4.5 Fatigue Life, Weld-Toe Stress Concentration & Paris-Erdogan Crack Growth 4.6 LEFM Fracture Toughness, Ductile-Brittle Transition & Larson-Miller Creep 4.7 Comparative Failure-Mode Synthesis & Integrated Flaw and Creep Assessment
6 Chapter 5: Heat Transfer & Fluid Mechanics in Welding
5.1 Fourier Conduction, Rosenthal Moving Heat Source & 2D vs. 3D Heat Flow 5.2 Adams Cooling Rate, the t8/5 Window & HAZ Peak-Temperature Distribution 5.3 Convection, Stefan-Boltzmann Radiation & Emissivity of Weld Surfaces 5.4 Arc Radiation Losses, Preheat Maintenance & PWHT Boundary Conditions 5.5 Fluid Statics, Bernoulli, Viscosity & Reynolds-Number Regimes 5.6 Gas Lens Mechanics, Buoyancy Effects & Torch Flow Design 5.7 Hyperbaric, Vacuum & Controlled-Atmosphere Welding Environments
7 Chapter 6: Electrical Engineering Principles for Welding Systems
6.1 DC and AC Waveforms, Polarity Thermodynamics & Welding Circuit Analysis 6.2 Joule Heating, Electrode Stickout Preheating & Circuit Voltage Distribution 6.3 Power Factor, Reactance, Impedance & Magnetic Transformer Principles 6.4 Lorentz Force, Electromagnetic Pinch Effect & Arc Blow
8 Chapter 7: Welding Heat Sources & Arc Physics
7.1 Volt-Ampere Characteristics, Operating Point, Self-Regulation & OCV Limits 7.2 Inductance, Slope Control & Dynamic Power-Source Response 7.3 Arc Fall Regions, Cathode Emission Mechanisms & Shielding-Gas Ionization 7.4 Maecker Plasma Jet, Degree of Ionization & Anode Heat Partitioning 7.5 Droplet Force Balance & Classification of Metal Transfer Regimes 7.6 Transition Current, Mode Comparison & Pulsed Waveform Design
9 Chapter 8: Arc Welding Processes & Parameter Controls
8.1 Shielded Metal Arc Welding (SMAW): Electrode Flux Chemistries & Variables 8.2 GMAW Process Physics, Transfer Modes & Shielding Gas Interactions 8.3 Solid, Metal-Cored & Flux-Cored Wires with CTWD and Parameter Envelopes 8.4 Gas Tungsten (GTAW) & Plasma Arc Welding (PAW): Electrodes & Keyholing 8.5 Submerged Arc Welding (SAW): Flux Basicity, Multi-Wire & High-Deposition Systems
10 Chapter 9: Advanced, Resistance & Solid-State Joining Processes
9.1 High-Energy-Density Beam Physics & Electron Beam Welding 9.2 Laser Beam Welding, EBW/LBW Comparison & Fiber Laser Parameter Derivation 9.3 Resistance Welding Physics, Electrode Materials & Spot Weld Sequence 9.4 Nugget Sizing, Seam and Projection Welding, and Lobe Curve Process Windows 9.5 Solid-State Joining: Friction Stir Welding (FSW), Explosion & Diffusion 9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc 9.7 High-Frequency, Flash, Stud & Ultrasonic Welding; Surfacing and Thermal Spray
11 Chapter 10: Physical & Transformation Metallurgy of Steels
10.1 Fe-Fe3C System, Crystal Lattices, c/a Ratio & Interstitial Solubility 10.2 Critical Temperatures, Invariant Reactions & the Lever Rule 10.3 Alloying Elements, the Gamma Loop & Phase-Fraction Calculations 10.4 TTT and CCT Diagrams, Constitutional Supercooling & Scheil Microsegregation 10.5 Non-Equilibrium Transformation Products & Martensite Modeling 10.6 HAZ Anatomy, Microstructural Sub-Zones & Multi-Pass Reheated Regions 10.7 HAZ Hardness Traverses, Toughness Gradients & Peak-Temperature Control
12 Chapter 11: Weldability, Cracking Mechanisms & Alloy Metallurgy
11.1 Hydrogen Cracking Conditions, Carbon Equivalent & Diffusible Hydrogen Control 11.2 Preheat, Interpass and Post-Heat Calculations for Cold-Crack Prevention 11.3 Solidification Cracking, Bead Aspect Ratio, Liquation & Lamellar Tearing 11.4 Lamellar Tearing Mitigation & Hot-Cracking Susceptibility Evaluation 11.5 Stainless Families, Schaeffler and WRC-1992 Diagrams, Ferrite Number & Sensitization 11.6 Duplex Stainless Metallurgy & Dissimilar-Metal Ferrite Prediction 11.7 Aluminum Oxide and Porosity Control, and Titanium Reactive-Metal Welding 11.8 Nickel Superalloys, Strain-Age Cracking & Guinier-Preston Aging Sequences
13 Chapter 12: Weldment Design, Stress Analysis & Joint Mechanics
12.1 AWS A2.4 Welding Symbol Anatomy, Symbol Library & Dimension Syntax 12.2 Joint Architecture, CJP versus PJP, and NDE Examination Symbols 12.3 Fillet and Groove Weld Sizing under Direct Stress in ASD and LRFD 12.4 Plug and Slot Welds, Stress Gradients & the Fillet Weld Break Test 12.5 Eccentric Loading Analysis: Elastic Vector Method vs Instantaneous Center 12.6 Fatigue Design of Welded Connections & Residual Stress/Distortion Control
14 Chapter 13: Non-Destructive Examination (NDE) & Discontinuity Analysis
13.1 Visual Testing Gages & Liquid Penetrant Capillary Mechanics 13.2 Magnetic Particle Testing: Flux Leakage, Field Geometry & Prod Amperage 13.3 Radiographic Physics, Geometric Unsharpness, Density & IQI Sensitivity 13.4 Computed and Digital Radiography & Radiographic Discontinuity Interpretation 13.5 Acoustic Wave Mechanics, Refraction & Angle-Beam Sound-Path Geometry 13.6 AWS D1.1 Decibel Rating, Phased Array & Time-of-Flight Diffraction
15 Chapter 14: Brazing, Soldering & Industrial Welding Safety
14.1 Brazing Thermodynamics, Capillary Wetting Physics & Joint Clearance 14.2 AWS A5.8 Brazing Filler Metals, FB Fluxes & Industrial Heating Processes 14.3 Soldering Fundamentals, Flux Chemistries & Intermetallic Formation 14.4 Hierarchy of Controls, Electric Shock Physics & Industrial Ventilation 14.5 Fume Exposure Limits, Arc Radiation, Hot Work and Confined-Space Entry 14.6 Arc-Generated Toxic Gases, Moving-Equipment Hazards & TWA Exposure Calculation
16 Chapter 15: Structural Fabrication & AWS D1.1 Code Implementation
15.1 AWS D1.1 Scope, Prequalification Limits, Base-Metal Groups & Matching Filler 15.2 Prequalified Joint Details, Backing Systems & Joint Specification Verification 15.3 Thermal Cut Edges, Fit-Up Tolerances & Minimum Preheat Requirements 15.4 Preheat Application Zones, Measurement Instrumentation & Fabrication Audits 15.5 PWHT Fundamentals, D1.1 Thermal Cycles & Visual Acceptance Criteria 15.6 D1.1 Nondestructive Examination Protocols, PWHT Scheduling & Visual Audit Practice
17 Chapter 16: Welding Procedure Qualification (WPS & PQR) per ASME IX & AWS B2.1
16.1 PQR versus WPS Hierarchy, Qualification Workflow & Standard Procedures 16.2 Manufacturer Responsibility, Subcontracting Limits & Multi-Process Qualification 16.3 Essential, Supplementary Essential and Nonessential Variables with Heat Input Mechanics 16.4 Waveform-Controlled Power Sources, Appendix H & Heat-Input Compliance 16.5 P-Numbers, Group Numbers, F-Numbers & A-Numbers 16.6 QW-451 Mechanical Test Protocols & Procedure Qualification Test Evaluation
18 Chapter 17: Filler Metal Specifications, Selection & Consumable Control
17.1 AWS A5 Architecture: SMAW, GMAW/GTAW and FCAW Consumable Classifications 17.2 SAW Wire-Flux Systems, Alloy Pickup & PWHT Property Effects 17.3 Stainless Filler Specifications, Solidification Modes & Dissimilar-Metal Joints 17.4 AWS A5.10 Aluminum Filler Selection & Dilution and Ferrite-Number Calculations 17.5 Consumable Storage, Conditioning Envelopes & Atmospheric Exposure Limits 17.6 Low-Hydrogen Designators, the Yurioka Parameter & Preheat Sizing
19 Chapter 18: Welder Performance Qualification, Quality Management & Welding Economics
18.1 Welder Qualification Philosophy, Test Positions & Thickness and Diameter Ranges 18.2 F-Number Hierarchy, Operator Qualification & Continuity Requirements 18.3 ISO 3834, Welding Coordination, Inspection Test Plans & Equipment Validation 18.4 EN 10204 Material Certification, Traceability & Heat-Input Nonconformance Auditing 18.5 Weld Cost Anatomy, Deposition Rates, Operating Factor & the Overwelding Law 18.6 Economic Optimization Strategies & Fabrication Cost Comparison
9.6 Thermal Cutting & Gouging: Oxyfuel, Plasma Arc and Air Carbon Arc
Key Takeaways Explain This Topic AI
Oxyfuel cutting is a chemical oxidation process: preheat raises steel to its kindling temperature near 870 degrees Celsius and the oxygen jet then burns iron exothermically.
Oxyfuel cutting works only where the metal oxide melts below the metal itself, which is why it cuts carbon and low-alloy steel but not stainless steel, aluminum or copper.
Plasma arc cutting uses a constricted transferred arc and cuts any electrically conductive metal, including stainless steel and aluminum, that oxyfuel cannot cut.
Air carbon arc gouging melts metal with a carbon electrode arc and blows it clear with a compressed air jet at roughly 80 to 100 psi.
A carbon-enriched layer is left after air carbon arc gouging and must be removed by grinding before welding, or it will produce a hard, crack-prone deposit.
Last updated: September 2026
Why Cutting Sits in the Welding Body of Knowledge
Thermal cutting determines joint preparation quality, and joint preparation quality determines weld quality. AWS D1.1 governs thermally cut edges as strictly as it governs welds, with limits on surface roughness and notch depth and a requirement to remove damaged material. A welding engineer specifies the cutting process, the edge quality, and the post-cut conditioning.
- Oxyfuel Gas Cutting (OFC)
- The Chemistry
Oxyfuel cutting is not melting. It is controlled rapid oxidation . A preheat flame raises a starting point on the steel to its kindling temperature — approximately 870 degrees Celsius (1600 degrees Fahrenheit) , a bright red heat — and a high-purity oxygen jet is then released. The iron burns: 3 Fe + 2 O 2 → Fe 3 O 4 + heat 3\,\text{Fe} + 2\,\text{O}_2 \rightarrow \text{Fe}_3\text{O}_4 + \text{heat} 3 Fe + 2 O 2 → Fe 3 O 4 + heat
The reaction is strongly exothermic and supplies most of the energy that sustains the cut; the preheat flame mainly maintains the leading edge. The oxygen jet simultaneously blows the molten oxide slag out of the kerf.
The Three Conditions for a Metal to Be Oxyfuel Cuttable
The metal must oxidise exothermically in an oxygen jet.
The oxide melting point must be below the metal melting point , so the oxide flows out of the kerf instead of forming a refractory crust.
The metal's thermal conductivity must be low enough that the cut zone stays above kindling temperature.
Carbon and low-alloy steels satisfy all three. Three important families do not:
- Metal Why oxyfuel cutting fails
- Stainless steel Chromium oxide is refractory and melts far above the steel, forming a protective crust
- Aluminum Aluminum oxide melts above 2000 degrees Celsius, far above the metal itself
- Copper and brass Very high thermal conductivity carries heat away faster than the reaction supplies it
Stainless steel can be forced with powder injection or a waster plate, but the accepted engineering answer is to use plasma arc cutting instead.
Fuel Gases
- Fuel gas Approximate neutral flame temperature Characteristics
- Acetylene ~3160 degrees Celsius Fastest preheat and pierce; unstable above 15 psig
- Propylene ~2900 degrees Celsius Good compromise; higher total heat than acetylene
- Propane ~2830 degrees Celsius Cheap, high total heat, slow pierce
- Natural gas ~2770 degrees Celsius Cheapest, slowest pierce, good for long production cuts
Acetylene has the highest primary-cone flame temperature and therefore the fastest pierce, which is why it dominates manual and repair cutting; the hydrocarbon fuels carry more total heat in the secondary envelope and suit long mechanised cuts.
Cut Quality
Drag lines on the cut face record the relationship between travel speed and oxygen flow. Vertical, evenly spaced drag lines indicate correct speed; heavy trailing drag lines indicate excessive travel speed and risk an incomplete cut at the bottom. Excessive preheat rounds the top edge; insufficient oxygen purity leaves adherent dross. AWS D1.1 sets roughness and notch-depth limits on thermally cut edges and requires that gouges beyond the limit be repaired.
Plasma Arc Cutting (PAC)
Plasma arc cutting uses a constricted transferred arc between a tungsten or hafnium electrode and the workpiece. The orifice constricts the plasma column, raising its temperature and velocity dramatically; the jet melts the metal and blows it out of the kerf by momentum rather than by chemical reaction.
Because the mechanism is melting and ejection rather than oxidation, plasma cuts any electrically conductive metal : stainless steel, aluminum, copper, nickel alloys and carbon steel alike. That is its decisive advantage over oxyfuel.
- Attribute Oxyfuel (OFC) Plasma (PAC)
- Mechanism Exothermic oxidation Melting and momentum ejection
- Materials Carbon and low-alloy steel only Any conductive metal
- Thin material speed Slow Very fast
- Heavy section capability Excellent, several hundred millimetres Limited by torch rating
- Kerf Wider, square Narrower, slight bevel
- Heat-affected zone Wider Narrower
- Equipment cost Low Higher
Two metallurgical cautions apply. Plasma cutting with nitrogen or air can nitride the cut face on stainless and duplex steels, and the nitrogen-enriched layer should be removed before welding. On aluminum, the cut face oxidises immediately and must be cleaned before welding as with any other preparation method.
Air Carbon Arc Gouging (CAC-A)
Air carbon arc gouging strikes an arc between a copper-coated carbon-graphite electrode and the work, melting the metal, then blows the molten pool clear with a compressed air jet issuing from the holder at approximately 80 to 100 psi . It removes metal rather than joining it.
Principal applications:
Backgouging the root of a double-sided groove weld to sound metal before welding the second side.
Defect removal — excavating cracks, slag and porosity for repair.
Removing temporary attachments , lugs and run-off tabs.
Bevelling heavy sections where a machined edge is not required.
The Carbon Pickup Problem
The graphite electrode leaves a thin carbon-enriched layer on the gouged surface. If a weld is deposited directly onto it, that carbon dissolves into the weld metal, raising local hardenability and producing a hard, crack-prone deposit. Codes therefore require the gouged surface to be ground clean to bright metal before welding. The same requirement arises if the air jet is inadequate or lags the arc: the pool is not cleared, carbon is trapped, and an irregular gouge profile results.
Air carbon arc gouging is also the noisiest and among the highest fume-generating operations in a fabrication shop, and it produces intense arc radiation. Local exhaust ventilation and full protective equipment are mandatory under ANSI Z49.1.
Exam Trap 1: "Oxyfuel cutting melts the steel." It does not. Oxyfuel cutting burns the steel in an oxygen jet, and the exothermic reaction supplies most of the cutting energy. This is exactly why it cannot cut stainless steel, aluminum or copper.
Exam Trap 2: Welding directly over an air carbon arc gouge. The carburized layer must be ground away first. Skipping that step is one of the most common causes of unexplained hardness and cracking in repair welds.
Exam Trap 3: Choosing oxyfuel for stainless because it is cheaper. Chromium oxide is refractory and forms a protective crust. Plasma arc cutting is the correct process for stainless, and no adjustment of oxygen pressure will change the oxide chemistry.