9.3 Clause 8 — Inspection and Acceptance Criteria

AWS CWI Certified Welding Inspector Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction to the AWS CWI Certification

What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application

2 1. Welding Processes and Fundamentals

1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables

3 2. Welding Metallurgy and Heat Control

2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress

4 3. Weld Discontinuities and Defects

3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile

5 4. Nondestructive Examination (NDE) Methods

4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)

6 5. Welding Symbols and Terminology

5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology

7 6. WPS, PQR, and Welder Qualification

6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)

8 7. Destructive Testing Methods

7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing

9 8. Welding Safety and Inspector Duties

8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations

10 9. AWS D1.1 Code Application (Part C)

9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation

11 10. Exam Strategies and Comprehensive Review

10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions

9.3 Clause 8 — Inspection and Acceptance Criteria

Key Takeaways Explain This Topic AI

Clause 8 defines inspector qualifications (CWI/SCWI/CAWI per QC1) and acceptance criteria; NDT personnel must hold ASNT certification (2025)

Inspector verifies before (WPS, qualifications, fit-up), during (preheat, amps/volts, technique), and after welding (size, profile, NDT, records)

Table 8.1: cracks never permitted; complete fusion required; craters filled to full size

Undercut: ≤1/32 in static general; ≤0.01 in for cyclic primary members transverse to tensile stress; ≤1/16 in for base metal ≥1 in

Fillet convexity max 1/16 in (face ≤5/16 in) or 1/8 in (larger); profiles per Clause 7.23 / Figure 7.4

VT on 100% of welds; RT/UT (Table 8.2) on specified CJP groove welds; repairs re-inspected by the same NDT method

Last updated: September 2026

The Inspector's Tasks Under Clause 8

Clause 8 is the working heart of the code for a CWI and the most-referenced clause on Part C. It defines who may inspect, what they must verify, and the accept/reject criteria for visual and nondestructive examination. The code distinguishes the Contractor's Inspector (Fabrication/Erection Inspector) from the Verification Inspector (often the Owner's), but when the term Inspector is used without qualification, the requirement applies to both.

Visual inspection must be performed by an individual qualified as a CWI or SCWI , or by an associate ( CAWI ) working under their direction, per AWS QC1 . In the 2025 edition, NDT personnel must hold ASNT certification (SNT-TC-1A / CP-189 basis) — closing earlier ambiguity. The Inspector's verification duties span the whole job:

Stage Inspector verification tasks

Before welding Approved WPS/PQR on hand; welder/operator qualifications current; base metal, filler, and consumable storage/identification correct; joint fit-up, root opening, alignment, cleanliness

During welding Preheat/interpass temperature; amperage/voltage/travel within WPS (calibrated meter); technique, position, interpass cleaning; correct electrode/flux

After welding Weld size and length, profile and contour, surface discontinuities; arc strikes; that NDT was done and dispositioned; documentation/records

The Inspector also verifies that calibration of inspection tools and NDT equipment is current and maintains inspection records .

Table 8.1 — Visual Acceptance Criteria (Verified Values)

Table 8.1 gives different limits for statically loaded nontubular versus cyclically loaded nontubular connections. Cyclic (fatigue) service is always as strict or stricter .

  • Discontinuity Statically loaded Cyclically loaded
  • Cracks Not permitted, any size/location Not permitted, any size/location
  • Weld/base-metal fusion Complete fusion required Complete fusion required
  • Crater cross section Craters filled to full weld size Craters filled to full weld size

Undercut (base metal <1 in) Depth ≤1/32 in [1 mm] general* ≤0.01 in [0.25 mm] in primary members transverse to tensile stress; otherwise ≤1/32 in

  • Undercut (base metal ≥1 in) Depth ≤1/16 in [2 mm] Same plus the cyclic transverse limit
  • Weld profile Per Clause 7.23 / Figure 7.4 Per Clause 7.23 / Figure 7.4

*Undercut exceptions for static loading: on welds ≥12 in [300 mm] , up to 1/16 in [2 mm] deep undercut is allowed for an accumulated length up to 2 in [50 mm] in any 12 in; on welds <12 in , accumulated undercut with depth no greater than 1/16 in may not exceed weld length × 0.16 . This wording incorporates AWS D1.1/D1.1M:2025 Amendment 1 (February 2026) , which corrected the depth qualification.

Porosity Limits (Often Misquoted)

Visual piping porosity acceptance also splits by loading:

CJP butt groove welds transverse to tensile stress: no visible piping porosity (static and cyclic).

Fillet/other groove welds (static): sum of pore diameters ≤3/8 in [10 mm] in any linear inch ; for welds ≥12 in, ≤3/4 in [20 mm] per 12 in .

Fillet welds generally: frequency ≤1 pore per 4 in [100 mm] , max diameter ≤3/32 in [2.5 mm] .

Weld Profiles and Reinforcement

Profiles are governed by Clause 7.23 and Figure 7.4 (renumbered from the older 7.1). Fillet faces may be slightly convex, flat, or slightly concave; maximum convexity is 1/16 in [2 mm] for faces up to 5/16 in [8 mm], and 1/8 in [3 mm] for larger faces . Concavity is allowed only while the effective throat still meets the specified size. Groove (butt) weld face reinforcement is limited (commonly to about 1/8 in [3 mm] for welds under 1 in), and reinforcement must blend smoothly with no overlap.

When NDT Beyond VT Is Required

  • Method When
  • VT 100% of all welds unless the Engineer specifies otherwise
  • RT / UT CJP groove welds where required by contract/Engineer (e.g., cyclically loaded tension joints)
  • MT / PT When specified by contract documents or the Engineer

UT acceptance uses Table 8.2 , scoring an indication by its indication rating (dB) versus weld thickness, with a length/severity class. RT rejects all cracks, limits elongated indications (slag, incomplete fusion) by length, and limits rounded indications (porosity) by the porosity charts.

Repair and Re-Inspection

When a weld is rejected, the Inspector documents it; repair follows an approved WPS; gouged areas (e.g., air carbon arc ) are ground smooth before rewelding; and the repair is re-examined by the same NDT method(s) used originally.

Static vs. Cyclic: Why the Limits Differ

The split between statically loaded and cyclically loaded acceptance is not arbitrary — it reflects fatigue . A statically loaded member sees essentially constant load; a small surface notch like shallow undercut rarely propagates. A cyclically loaded member (crane runways, bridges, equipment supports) sees thousands to millions of stress reversals, and a notch transverse to the tensile stress becomes a fatigue crack initiation site . This is why undercut acceptance depends on the member, loading category, and stress direction. Use the corresponding row and column in Table 8.1, including its qualifications, rather than treating the general static limit as a universal allowance.

On Part C, the giveaway words are "cyclically loaded," "fatigue," "transverse to tensile stress," or "primary member" — they pull you to the stricter column.

Surface Discontinuities the Inspector Names

Visual inspection is pattern recognition plus measurement. Know the A3.0 terms and which are categorically rejectable:

  • Discontinuity Definition D1.1 visual treatment
  • Crack Fracture-type, sharp tip Never acceptable, any size
  • Incomplete fusion Weld did not fuse to base/prior bead Never acceptable
  • Overlap Weld metal protruding past the toe without fusion Rejectable (a profile defect)
  • Undercut Groove melted into base metal at the toe Limited per Table 8.1
  • Porosity Gas-pocket cavity Limited by type/size/frequency
  • Underfill / undersize Weld below specified size Limited per fillet-undersize rules
  • Arc strike Localized melting outside the joint Must be evaluated/ground; can cause hard spots
  • Timing of Inspection (A Hidden Trap)

Visual inspection timing matters for quenched-and-tempered steels. Most steels are inspected after cooling to ambient , but ASTM A514, A517, and A709 Grade HPS 100W [HPS 690W] must wait at least 48 hours after weld completion before final inspection, because delayed (hydrogen) cracking can appear hours later. A weld that looked good immediately may crack overnight, so the code mandates the wait.

Documentation and Authority

The Inspector's accept/reject authority is real but bounded: the CWI applies the code and contract criteria and cannot unilaterally waive them — only the Engineer can authorize a deviation. The Inspector documents inspections, marks rejected areas, verifies that repairs follow an approved WPS, and confirms re-examination by the same NDT method . Clean, contemporaneous records are part of the job, not an afterthought.

For the Exam: Table 8.1 is the single most-tested table. Lock in: cracks are never acceptable , the 0.01 in cyclic undercut limit on transverse primary members, and that complete fusion is always required.