3.2 Cracks — Types, Causes, and Significance

AWS CWI Certified Welding Inspector Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction to the AWS CWI Certification

What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application

2 1. Welding Processes and Fundamentals

1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables

3 2. Welding Metallurgy and Heat Control

2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress

4 3. Weld Discontinuities and Defects

3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile

5 4. Nondestructive Examination (NDE) Methods

4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)

6 5. Welding Symbols and Terminology

5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology

7 6. WPS, PQR, and Welder Qualification

6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)

8 7. Destructive Testing Methods

7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing

9 8. Welding Safety and Inspector Duties

8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations

10 9. AWS D1.1 Code Application (Part C)

9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation

11 10. Exam Strategies and Comprehensive Review

10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions

3.2 Cracks — Types, Causes, and Significance

Key Takeaways Explain This Topic AI

Cracks are planar and prohibited by AWS D1.1 regardless of size or location — zero tolerance

Hot cracks form at high temperature from low-melting S/P films at grain boundaries (centerline/liquation)

Cold/hydrogen cracking needs hydrogen + martensitic microstructure + tensile stress, and is delayed

Crater cracks are star-shaped terminations prevented by crater-fill technique

  • Lamellar tearing is a base-metal step-like failure in rolled plate under through-thickness strain
  • Last updated: June 2026

The Most Serious Discontinuity

The reason is mechanical: a crack has an extremely sharp tip, producing the highest stress-concentration factor of any discontinuity, so it can propagate under static, cyclic, or impact loading toward brittle fracture. You should also know that cracks are categorized by where they sit relative to the weld — weld-metal cracks lie within the deposited metal, while base-metal cracks lie in the heat-affected zone or unaffected base metal — because the cause and corrective action differ for each. 1 always rejectable.

Classification by Temperature

Type When it forms Mechanism Typical location

Hot crack During/just after solidification (high temperature) Low-melting liquid films at grain boundaries can't sustain shrinkage strain Weld metal centerline; partially-melted HAZ

Cold crack (HIC / hydrogen / delayed) After cooling, often hours/days later, near or below ~200–400°F Hydrogen + hard microstructure (martensite) + tensile stress HAZ (underbead), weld toe, root

Reheat (stress-relief) crack During PWHT or high-temperature service Stress-relaxation cracking in coarse-grained HAZ of certain Cr-Mo-V alloy steels Coarse-grained HAZ

Lamellar tear During/after welding Through-thickness tensile strain on plate with planar inclusions Base metal, parallel to rolling plane

Classification by Location and Orientation

  • Crack Description Common mechanism
  • Longitudinal Parallel to the weld axis Solidification (centerline) hot crack or transverse shrinkage HIC
  • Transverse Perpendicular to the weld axis Usually hydrogen (HIC) from longitudinal shrinkage stress
  • Crater crack Star/X-shaped at the end of a bead Solidification shrinkage in the crater depression
  • Toe crack Initiates at the weld toe into the HAZ HIC or fatigue; toe is a stress-concentration site
  • Root crack At the weld root HIC, hot crack, or extension of incomplete penetration
  • Underbead crack In the HAZ beneath the bead, not surface-breaking Classic hydrogen (HIC) signature
  • Throat crack Through the throat of a fillet weld, longitudinal Hot or cold; high-restraint fillets
  • Hot Cracking — Mechanism

Solidification (centerline) cracking occurs as the weld pool freezes. Elements such as sulfur and phosphorus form low-melting-point eutectic films that remain liquid at grain boundaries after the bulk has solidified. As the weld contracts, these liquid films cannot carry the tensile shrinkage strain and a crack opens. A deep, narrow bead ( high depth-to-width ratio ) drives impurities to the centerline and promotes this crack. Liquation cracking is the HAZ cousin: partially melted grain boundaries open under strain, common in austenitic stainless and nickel alloys.

Controls: keep S and P low, avoid deep narrow beads, lower heat input, and (for stainless) target a few percent ferrite in the weld metal.

Cold (Hydrogen-Induced) Cracking — Three Factors

HIC requires three conditions simultaneously; remove any one and it cannot occur:

Diffusible hydrogen — from moisture in flux/coating, oil, grease, paint, rust, or humid air.

Susceptible (hard) microstructure — typically martensite formed by fast cooling of higher-carbon/alloy steel.

Tensile stress / restraint — from shrinkage, fixturing, and section thickness, concentrated at notches like the weld toe.

It is delayed — it can appear hours after welding once hydrogen diffuses, which is why critical welds are sometimes held before final inspection. Controls: preheat and control interpass temperature (slows cooling, lets hydrogen diffuse out, avoids martensite), use low-hydrogen electrodes stored in rod ovens, clean the joint, and reduce restraint. Higher-carbon and alloy steels with elevated carbon equivalent (CE) are most prone, because they harden readily on fast cooling; the CE value is a key driver of the required preheat.

The delayed nature is a classic exam point — a weld can pass visual inspection immediately yet crack overnight, so HIC is sometimes called delayed cracking .

Crater Cracks and Lamellar Tearing

Crater cracks form where the welder breaks the arc: the crater cools fast with a high surface-to-volume ratio, and multidirectional shrinkage opens a star crack. Prevent them with proper crater-fill technique (pause, backstep, or use a crater-fill control). Lamellar tearing is a step-like separation in rolled plate loaded in the through-thickness (Z) direction, exploiting elongated sulfide/silicate inclusions parallel to the rolling plane (common in T- and corner joints).

Controls: specify Z-quality (through-thickness tested) steel , use low-sulfur plate, redesign to reduce through-thickness strain, and apply buttering layers.

Exam essentials: Cracks are essentially never acceptable under AWS D1.1. Distinguish hot (solidification, S/P films, high temperature) from cold/HIC (hydrogen + martensite + stress, delayed, underbead/toe). Crater cracks are the most common preventable type; lamellar tearing is a base-metal failure, not a weld-metal failure.

Crack Types the Exam Tests

Beyond the temperature classification, the CWI must place each named crack with its dominant mechanism and location, because cause and corrective action differ:

Crack Family Dominant cause

Solidification / centerline (hot) Hot Low-melting S/P eutectic films at grain boundaries; worsened by high depth-to-width bead ratio

Crater crack Hot (shrinkage) Arc broken without crater fill; multidirectional shrinkage of the crater depression

Hydrogen-induced (cold/delayed) Cold Diffusible hydrogen + hard microstructure + tensile stress, appearing hours after welding

Underbead / toe / root crack Cold (usually) HIC signatures in the HAZ; toe and root are stress-concentration sites

Lamellar tearing Base-metal Through-thickness (Z-direction) strain exploiting planar sulfide/silicate inclusions in rolled plate

  • Reheat (stress-relief) Service/PWHT Stress relaxation in coarse-grained HAZ of certain Cr-Mo-V steels
  • The Three Conditions for Hydrogen-Induced Cracking

HIC — also called cold cracking or delayed cracking — requires three conditions simultaneously , and removing any one prevents it. This is one of the most heavily tested points in welding metallurgy:

Diffusible hydrogen — from moisture in flux or electrode coating, oil, grease, paint, rust, or humid air.

Susceptible (hard) microstructure — typically martensite formed when higher-carbon or high-carbon-equivalent steel cools too fast through the transformation range.

Tensile stress / restraint — from weld shrinkage, fixturing, and section thickness, concentrated at notches such as the weld toe.

The standard controls each attack one leg of that triangle: preheat and interpass temperature slow cooling so hydrogen diffuses out and martensite is avoided; low-hydrogen electrodes stored in rod ovens and clean joints remove the hydrogen source; and joint redesign reduces restraint. Steels with elevated carbon equivalent (CE) harden readily on fast cooling, so CE is the key driver of the required preheat. The delayed nature is the classic trap: a weld can pass visual inspection immediately and still crack overnight.

Cracks Are Prohibited Regardless of Size

Under AWS D1.1 , cracks are essentially never acceptable — any crack of any length, in the weld metal or the HAZ, is a reject regardless of size. There is no aggregate-length or size allowance the way there is for porosity or slag. The mechanical reason is that a crack has the sharpest possible tip and the highest stress-concentration factor of any discontinuity, so it can propagate under static, cyclic, or impact loading toward brittle fracture. That is why crack-prevention controls — preheat, low-hydrogen practice, crater fill, and Z-quality steel for through-thickness loading — are emphasized so heavily in code work.