Study guide
3.3 Porosity and Inclusions
AWS CWI Certified Welding Inspector Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction to the AWS CWI Certification
What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application
2 1. Welding Processes and Fundamentals
1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables
3 2. Welding Metallurgy and Heat Control
2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress
4 3. Weld Discontinuities and Defects
3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile
5 4. Nondestructive Examination (NDE) Methods
4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)
6 5. Welding Symbols and Terminology
5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology
7 6. WPS, PQR, and Welder Qualification
6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)
8 7. Destructive Testing Methods
7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing
9 8. Welding Safety and Inspector Duties
8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations
10 9. AWS D1.1 Code Application (Part C)
9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation
11 10. Exam Strategies and Comprehensive Review
10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions
3.3 Porosity and Inclusions
Key Takeaways Explain This Topic AI
Porosity is gas trapped during solidification; inclusions are trapped solids — both are volumetric
Four porosity types: uniformly scattered, cluster, linear, and piping (wormholes)
Wind is the #1 outdoor GMAW porosity cause; inadequate interpass cleaning is the #1 slag-inclusion cause
Tungsten inclusions occur in GTAW when the electrode touches the pool; they read bright on radiographs
- AWS D1.1: CJP butt welds transverse to tensile stress permit NO visible piping porosity
- Last updated: September 2026
Volumetric Discontinuities
Porosity and inclusions are volumetric (three-dimensional, rounded) discontinuities — they occupy volume inside the weld rather than presenting a sharp planar face. Because their notch is blunt, they are generally less damaging than cracks or lack of fusion for the same size, but they are routinely the most frequently encountered discontinuities and will reject a weld once they exceed the code's size, frequency, or distribution limits. The CWI exam tests you on types, causes, and the most likely corrective action for a described situation.
Porosity
Per AWS A3.0, porosity is cavity-type discontinuities formed by gas entrapment during solidification. Dissolved gas (most commonly hydrogen, also nitrogen, oxygen, CO) tries to escape the freezing pool; if it is trapped before solidification, it leaves a rounded void.
Types of Porosity
Type Appearance Typical cause
Uniformly scattered Small pores evenly distributed through the weld General mild contamination of base metal or consumable
Cluster (localized) porosity A group of pores in one spot Localized contamination, poor arc starts/stops
Linear (aligned) porosity Pores in a row Contamination along a specific interface — root, tack weld, interpass line
Piping porosity (wormholes) Elongated tubular pores, axis roughly perpendicular to the weld face Gas (often from base-metal coatings/galvanizing or moisture) evolving and channeling during solidification
Causes of Porosity — Gas Source
- Cause Gas generated
- Moisture on plate, electrode coating, or flux Hydrogen / water vapor
- Oil, grease, paint on the joint Hydrogen, carbon compounds
- Rust or mill scale Oxygen, carbon monoxide
- Inadequate shielding-gas coverage / low flow Nitrogen, oxygen from air
- Wind or drafts disturbing the gas shield Atmospheric N₂/O₂
- Excessive arc length (SMAW/GMAW) Air entrainment into the arc
- Damp low-hydrogen flux/electrode (improper storage) Hydrogen
- Welding over porous tack welds Trapped gas from the tack
Match the observed clue to a possible gas source: Damp electrodes left out of the oven → hydrogen. Rust/scale not cleaned → oxygen/CO. Long arc → air entrainment. Porosity may be surface-breaking (visible during VT) or fully subsurface (often evaluated by RT, where rounded pores appear as darker indications; detection depends on the examination method and its sensitivity). Because the gas pocket is rounded, porosity is one of the more tolerable discontinuities — but clustered, linear, or piping porosity concentrated at the root or transverse to tension is treated far more strictly than the same volume of scattered pores.
Inclusions
An inclusion is solid foreign material entrapped in the weld metal or between passes — distinct from porosity, which is a gas cavity.
Inclusion Description Primary cause
Slag inclusion Nonmetallic solid (slag from a flux/coating process: SMAW, FCAW, SAW) trapped in the weld Inadequate interpass slag removal , too-fast travel letting slag run ahead of the puddle, undercut pockets, poor bead profile/sequence
Tungsten inclusion Particle of tungsten electrode embedded in the weld (GTAW only) Electrode dipped into the molten pool, or too much current for the tungsten diameter; shows as a bright spot on a radiograph (tungsten is dense)
Oxide inclusion Surface oxide (e.g., aluminum oxide) folded into the weld Inadequate shielding or surface cleaning, especially on aluminum
Slag-inclusion prevention is a recurring exam point: remove all slag between every pass (chip, wire-brush, or grind); use a proper bead sequence so you don't create sharp valleys that trap slag; keep travel speed correct so slag does not solidify ahead of the molten metal; and manipulate the arc to keep slag floating behind the puddle. Tungsten-inclusion prevention: keep the tungsten out of the pool (proper arc length and technique) and size the electrode to the amperage.
Acceptance Criteria — AWS D1.1 Clause 8
Visual and volumetric limits differ for statically versus cyclically loaded connections, with cyclic (fatigue) members held to tighter limits.
- Condition (per AWS D1.1) Limit
- CJP groove welds in butt joints transverse to computed tensile stress No visible piping porosity
Other groove welds and fillet welds Sum of visible piping porosity ≥ 1/32 in. diameter ≤ 3/8 in. in any linear inch , and ≤ 3/4 in. in any 12 in. of weld
Fillet welds — piping porosity frequency ≤ one in each 4 in. of length; max diameter ≤ 3/32 in.
Subsurface slag and porosity in radiographically or ultrasonically tested welds are judged against Clause 8 RT/UT tables based on size and spacing. The big idea: rounded, well-distributed porosity is tolerated within limits; concentrated, aligned, or transverse-tension piping porosity is treated most harshly.
Exam essentials: Porosity = trapped gas ; inclusions = trapped solid . Wind is the #1 outdoor GMAW porosity cause; inadequate interpass cleaning is the #1 slag cause; tungsten in the pool causes tungsten inclusions (GTAW). Know that CJP butt welds transverse to tension permit no visible piping porosity.
Porosity Types, Inclusion Types, and D1.1 Numbers
The CWI must name each porosity pattern, map it to a gas source, and recall the D1.1 acceptance numbers for piping porosity. Pulling the key facts together:
Porosity Patterns and Gas Sources
- Pattern Look Gas source clue
- Uniformly scattered Small pores spread through the weld General contamination of base metal or consumable
- Cluster (localized) A group of pores in one spot Poor arc starts/stops, localized contamination
- Linear (aligned) Pores in a row along an interface Contamination at the root, a tack, or an interpass line
Piping (wormhole) Elongated tubular pores, axis roughly perpendicular to the weld face Gas from base-metal coatings, galvanizing, or moisture channeling during freezing
The exam often gives a scenario and asks for the cause: damp electrodes out of the oven → hydrogen ; uncleaned rust or mill scale → oxygen / carbon monoxide ; wind or excessive arc length → atmospheric nitrogen / oxygen entrained into the arc. Porosity may be surface-breaking (caught in VT) or fully subsurface (read on RT as dark, well-rounded spots).
Inclusion Types
Slag inclusions — nonmetallic solid from a flux process (SMAW, FCAW, SAW) trapped by inadequate interpass cleaning, too-fast travel letting slag run ahead of the puddle, or sharp bead valleys. The #1 slag cause is inadequate interpass slag removal .
Tungsten inclusions — a particle of the GTAW electrode dropped into the pool, or too much current for the tungsten diameter; on a radiograph tungsten is dense, so it reads as a bright white spot (most other discontinuities read dark).
Oxide inclusions — surface oxide folded into the weld, common on aluminum with poor cleaning or shielding.
AWS D1.1 Acceptance for Piping Porosity
- Condition Limit
- CJP butt joints transverse to computed tensile stress No visible piping porosity
Other groove and fillet welds Sum of piping porosity ≥ 1/32 in. ≤ 3/8 in. per linear inch and ≤ 3/4 in. per 12 in.
Fillet welds — frequency ≤ one in each 4 in. of length; max diameter ≤ 3/32 in.
The governing idea: rounded, well-distributed porosity is tolerated within limits, but concentrated, aligned, or transverse-tension piping porosity is judged most harshly — and a CJP butt weld transverse to tension permits no visible piping porosity at all.