Study guide

2.4 Hydrogen-Induced Cracking (HIC)

AWS CWI Certified Welding Inspector Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction to the AWS CWI Certification

What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application

2 1. Welding Processes and Fundamentals

1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables

3 2. Welding Metallurgy and Heat Control

2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress

4 3. Weld Discontinuities and Defects

3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile

5 4. Nondestructive Examination (NDE) Methods

4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)

6 5. Welding Symbols and Terminology

5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology

7 6. WPS, PQR, and Welder Qualification

6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)

8 7. Destructive Testing Methods

7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing

9 8. Welding Safety and Inspector Duties

8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations

10 9. AWS D1.1 Code Application (Part C)

9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation

11 10. Exam Strategies and Comprehensive Review

10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions

2.4 Hydrogen-Induced Cracking (HIC)

Key Takeaways Explain This Topic AI

HIC requires THREE simultaneous conditions: susceptible (hard) microstructure + diffusible hydrogen + tensile stress

Remove any one condition and cracking cannot occur — this organizes every prevention method

HIC is delayed: forms below ~400°F and can appear 48–72 hours after welding, so codes may require a 48-hour hold before final NDE

Diffusible-hydrogen designators H4/H8/H16 = max mL of hydrogen per 100 g deposited; E7018-H4 is low-hydrogen, E6010 is high-hydrogen

Holding ovens (~250–300°F) keep electrodes dry; rebake ovens (~700–800°F) recondition them

  • Prevention: preheat, low-hydrogen consumables, clean dry joints, post-heat bake-out, PWHT, low restraint
  • Last updated: June 2026

The Most Dangerous Cracking Mechanism

Hydrogen-induced cracking (HIC) — also called cold cracking , delayed cracking , or underbead cracking — is the most common and most dangerous cracking mechanism in carbon and low-alloy steel welding. What makes it insidious is its delayed onset : it forms below about 400°F (200°C) and can appear hours or even days after welding is finished and the welder has left, often after the weld has already passed a visual inspection. For that reason it is the single most heavily tested cracking topic on the CWI exam.

The Three Required Conditions (All Must Be Present)

HIC is a classic "three-legged stool." It requires the simultaneous presence of all three conditions; remove any one and cracking cannot occur. Every prevention strategy is simply an attack on one or more of these legs.

Condition What It Means How It Is Controlled

1. Susceptible (hard) microstructure Martensite in the HAZ or weld Preheat, control heat input, lower carbon equivalent

2. Sufficient diffusible hydrogen Roughly > 4–8 mL per 100 g of deposited metal Low-hydrogen consumables, dry storage, clean joint

3. Adequate tensile stress Residual stress + restraint + applied load Lower restraint, joint design, PWHT/stress relief

Sources of Hydrogen

Hydrogen enters the molten weld pool as atomic hydrogen, dissolves while the metal is liquid and austenitic, and then becomes trapped as the weld solidifies and cools. The inspector must recognize and eliminate the sources.

Source Mechanism Prevention

Moisture in electrode coatings Cellulose/organic flux and absorbed water break down in the arc Use low-hydrogen electrodes; bake/store properly

  • Moisture in SAW flux Bonded/agglomerated flux absorbs humidity Dry flux per manufacturer instructions
  • Surface contaminants Oil, grease, paint, rust, moisture contain hydrogen Clean the joint before welding
  • Atmospheric humidity Damp air near the arc Shield the arc; do not weld in rain
  • Shielding-gas moisture Wet hoses or contaminated gas Use dry gas; check dew point

Low-Hydrogen Practice and Diffusible-Hydrogen Designators

Filler-metal specifications (AWS A5 series) assign optional diffusible-hydrogen designators that cap the hydrogen a consumable can contribute, expressed in milliliters of diffusible hydrogen per 100 grams of deposited weld metal :

  • Designator Maximum Diffusible Hydrogen Use
  • H16 16 mL / 100 g General work, low restraint
  • H8 8 mL / 100 g Moderate restraint / higher strength
  • H4 4 mL / 100 g High restraint, high-strength, offshore/nuclear code

A designation such as E7018-H4 means a low-hydrogen electrode that delivers no more than 4 mL/100 g — the most crack-resistant choice. By contrast, cellulosic electrodes (E6010/E6011) are deliberately high-hydrogen for deep penetration and are not low-hydrogen.

Electrode care is part of low-hydrogen practice and is an inspector check item:

Low-hydrogen electrodes (E7018) ship in hermetically sealed cans; once opened they absorb atmospheric moisture.

After opening, store in a holding oven at ~250–300°F (120–150°C) to keep them dry.

If exposed beyond the code/manufacturer limit (commonly a few hours), recondition (rebake) them, typically around 700–800°F (370–425°C) for one hour — never exceed the manufacturer maximum, which damages the flux binder.

A holding oven maintains dryness; a rebake oven restores it. Do not confuse the two temperatures.

Characteristics and Identification

  • Feature Description
  • Location Usually the HAZ (underbead/toe), can also be in weld metal
  • Orientation Often transverse (perpendicular to weld axis)
  • Timing Delayed — hours to days after welding
  • Temperature Forms below ~400°F (200°C) during cooling
  • Appearance Tight, sometimes microscopic; may not be visible at first

Prevention and the "Delayed" Nature

Because every prevention method targets one of the three required conditions, the inspector can reason about them systematically:

  • Strategy Leg Attacked
  • Preheat / maintained interpass Microstructure (less martensite) + hydrogen (lets it diffuse out)
  • Low-hydrogen consumables (H4/H8) Hydrogen
  • Proper electrode storage / rebake Hydrogen
  • Clean, dry joint surfaces Hydrogen
  • Post-heat (hydrogen bake-out), ~400–600°F held 1–2 h Hydrogen (drives it out before it cracks)
  • PWHT / stress relief Stress + tempers martensite (microstructure)
  • Lower-restraint joint design Stress

HIC is called delayed cracking because hydrogen is mobile in the steel lattice and needs time to (1) diffuse from the weld metal into the HAZ, (2) accumulate at high-stress sites such as grain boundaries and martensite interfaces, and (3) build enough local pressure to nucleate and propagate a crack. This sequence can take 48 to 72 hours . That delay is exactly why some codes and contracts require a minimum hold of 48 hours after welding before final NDE on certain high-strength or highly restrained joints — so any cracking has time to appear before the inspector signs off.

For the Exam: HIC is the #1 tested cracking topic. Memorize the three required conditions — susceptible microstructure + diffusible hydrogen + tensile stress — and that all three must be present simultaneously. Know that it is delayed (forms below 400°F, can appear up to 72 hours later) and that E7018-H4 is a low-hydrogen choice while E6010 is high-hydrogen.