Study guide

2.3 Preheat and Interpass Temperature

AWS CWI Certified Welding Inspector Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction to the AWS CWI Certification

What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application

2 1. Welding Processes and Fundamentals

1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables

3 2. Welding Metallurgy and Heat Control

2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress

4 3. Weld Discontinuities and Defects

3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile

5 4. Nondestructive Examination (NDE) Methods

4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)

6 5. Welding Symbols and Terminology

5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology

7 6. WPS, PQR, and Welder Qualification

6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)

8 7. Destructive Testing Methods

7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing

9 8. Welding Safety and Inspector Duties

8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations

10 9. AWS D1.1 Code Application (Part C)

9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation

11 10. Exam Strategies and Comprehensive Review

10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions

2.3 Preheat and Interpass Temperature

Key Takeaways Explain This Topic AI

Preheat slows cooling, lets hydrogen escape, lowers residual stress, and dries surface moisture

IIW CE = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15; higher CE = more hardenable = more preheat

CE < 0.35 excellent, 0.35–0.45 good, 0.45–0.55 fair, > 0.55 poor weldability

AWS D1.1 preheat (Table 5.8, formerly 3.2) is set by steel category, thickness, process, and hydrogen level

Measure preheat opposite the heated face, or at least one thickness / not less than 3 in. (75 mm) from the joint

  • Minimum interpass = minimum preheat; a maximum interpass (often ~400–600°F) protects toughness
  • Last updated: June 2026

Definitions and Purpose

Preheat is heat applied to the base metal before welding begins (and maintained during welding). Interpass temperature is the temperature of the weld zone between successive passes of a multi-pass weld — measured immediately before the next pass is started. Preheat maintenance temperature is the minimum that must be held throughout. These three controls govern the cooling rate and are the inspector's primary tools for preventing hydrogen-induced cracking and managing HAZ microstructure.

Preheat serves four purposes, all of which an inspector should be able to recite:

Slows the cooling rate through the 1,500–900°F range → less martensite → lower cracking risk.

Allows diffusible hydrogen to escape the weld and HAZ before it can accumulate.

Reduces residual stress by lowering the thermal gradient between the weld and the surrounding metal.

Drives off surface moisture (and condensation), removing a hydrogen source.

Carbon Equivalent (CE)

The carbon equivalent converts a steel's alloy chemistry into a single number that predicts its hardenability and cracking susceptibility — the higher the CE, the more preheat the steel needs. The most widely used formula is the IIW (International Institute of Welding) formula , where each element is its weight percent:

CE = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Manganese is the most significant alloying contributor after carbon (divided by 6). Chromium, molybdenum, and vanadium are grouped (divided by 5); nickel and copper are the weakest contributors (divided by 15). For thin sections and lower strengths, the Pcm formula is sometimes used instead, but the IIW CE is the one most CWI candidates are asked to apply.

  • CE Value Weldability Typical Action
  • < 0.35 Excellent Preheat usually not required
  • 0.35–0.45 Good Preheat may be required for thick sections
  • 0.45–0.55 Fair Preheat required; low-hydrogen practice essential
  • > 0.55 Poor High preheat + low-hydrogen + controlled procedure essential

Worked example: a steel with 0.18% C, 1.20% Mn, 0.10% Cr, 0.05% Mo, 0.20% Ni, 0.15% Cu gives CE = 0.18 + 1.20/6 + (0.10+0.05+0)/5 + (0.20+0.15)/15 = 0.18 + 0.20 + 0.03 + 0.023 ≈ 0.43 — "good," but preheat is prudent on thick sections.

AWS D1.1 Preheat Requirements

AWS D1.1, Structural Welding Code — Steel , specifies prequalified minimum preheat and interpass temperatures in a table (Table 5.8 in the 2020/2025 editions; the same content was Table 3.2 in older editions). The required temperature is selected from four inputs:

  • Steel category (steels grouped by ASTM specification and strength)
  • Thickness of the thickest part at the point of welding
  • Welding process and hydrogen level (e.g., SMAW with low-hydrogen electrodes vs. non-low-hydrogen)
  • Diffusible hydrogen designator of the consumable, under the alternative (Annex H) hydrogen-control method
  • Thickness of thickest part Typical minimum preheat (low-hydrogen process, common A36 / A572 Gr 50)
  • Up to 3/4" (20 mm) 32°F (0°C) — none required
  • Over 3/4" to 1-1/2" (20–38 mm) 50°F (10°C)
  • Over 1-1/2" to 2-1/2" (38–65 mm) 150°F (66°C)
  • Over 2-1/2" (65 mm) 225°F (107°C)

Higher-strength or higher-carbon steel categories, or use of non-low-hydrogen consumables, raise these values substantially. The exact numbers come from the code table on exam day (Part C is open-book), but the trend — preheat rises with thickness and with steel strength/hardenability — must be second nature.

Measuring Preheat and Interpass Temperature

Common measurement tools:

Temperature-indicating crayons (Tempilstik): rated to melt at a set temperature; a smear that liquefies confirms the minimum is met.

Contact pyrometer / surface thermocouple: gives a direct numerical reading.

Infrared (non-contact) thermometer: convenient but unreliable on shiny/scaled surfaces unless emissivity is corrected.

Where to measure (AWS D1.1): where the heating torch is applied to one side, measure on the surface opposite the heated face to confirm the full thickness is hot. Where heating one side and measuring the opposite face is not possible, after the heat source is removed, measure at a distance at least equal to the thickness of the thickest part but not less than 3 in. (75 mm) from the joint, allowing time for equalization. A localized torch reading taken right at the joint on the heated side overstates the temperature and is a classic exam trap.

Interpass Temperature

Interpass temperature has both a floor and a ceiling:

Minimum interpass = minimum preheat. The required preheat must be maintained between every pass; letting the joint cool below it reintroduces the cracking risk preheat was meant to prevent.

Maximum interpass temperature is imposed (by the WPS or code) to protect mechanical properties. Running too hot causes:

Excessive austenite grain growth in the HAZ (lower toughness)

Loss of strength and impact toughness, especially in quenched-and-tempered (Q&T) and thermomechanically-controlled-processed (TMCP) steels

Typical maximum interpass values fall around 400–600°F (200–315°C) , but Q&T steels may be capped lower to preserve their heat-treated properties.

The inspector's job is to verify, with a calibrated instrument and at the correct location, that the joint stayed between the WPS minimum and maximum throughout welding — and to document it.

For the Exam: Know the IIW CE formula cold and that higher CE means more preheat. Know that minimum interpass equals minimum preheat, that a maximum interpass exists to protect toughness, and the D1.1 measurement rule: opposite the heated face, or at least the thickness but not less than 3 in. (75 mm) from the joint.