Study guide

1.2 GMAW — Gas Metal Arc Welding (MIG/MAG)

AWS CWI Certified Welding Inspector Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction to the AWS CWI Certification

What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application

2 1. Welding Processes and Fundamentals

1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables

3 2. Welding Metallurgy and Heat Control

2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress

4 3. Weld Discontinuities and Defects

3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile

5 4. Nondestructive Examination (NDE) Methods

4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)

6 5. Welding Symbols and Terminology

5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology

7 6. WPS, PQR, and Welder Qualification

6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)

8 7. Destructive Testing Methods

7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing

9 8. Welding Safety and Inspector Duties

8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations

10 9. AWS D1.1 Code Application (Part C)

9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation

11 10. Exam Strategies and Comprehensive Review

10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions

1.2 GMAW — Gas Metal Arc Welding (MIG/MAG)

Key Takeaways Explain This Topic AI

GMAW feeds continuous solid wire with external gas on a constant-voltage (CV) source; wire-feed speed sets amperage

Four transfer modes: short-circuit (all-position, low heat), globular (flat, spatter), spray (≥80% Ar, high deposition), pulsed-spray (all-position, controlled heat)

MIG = inert gas (Ar/He); MAG = active gas (CO₂ or Ar/CO₂); C25 (75/25) is the common steel mix

Spray transfer requires ≥80% argon and current above the transition current (~220–250 A for 0.045" wire)

  • GMAW deposition efficiency is 90–95%, far above SMAW's 60–65%, but short-circuit mode risks cold lap
  • Last updated: June 2026

Gas Metal Arc Welding (GMAW)

Gas Metal Arc Welding (GMAW) — MIG (Metal Inert Gas) or MAG (Metal Active Gas) — is a semi-automatic process feeding a continuous solid wire electrode through a gun while an externally supplied shielding gas protects the pool. It dominates shop fabrication because it deposits fast (90–95% efficiency, no slag to chip) and is easily mechanized or robotized.

The gun's contact tip energizes the wire; the arc forms between wire and work; gas flows through the nozzle. The MIG/MAG distinction is purely about the gas:

MIG uses inert gas (argon, helium) — non-ferrous metals such as aluminum and (with additions) stainless.

MAG uses active gas (CO₂, or Ar + CO₂/O₂) — carbon and low-alloy steels. The small CO₂ or O₂ fraction is deliberately "active": it reacts in the arc to stabilize it and improve wetting, but it also oxidizes alloy, which is why steel wires carry extra silicon and manganese deoxidizers to compensate.

Power Source — Constant Voltage

GMAW uses a constant-voltage (CV) power source, the opposite of SMAW. The welder sets voltage and wire-feed speed; the CV supply self-regulates burn-off so the arc length stays constant. Wire-feed speed sets amperage — feed faster and current rises. This self-correcting "burnback" behavior is what makes GMAW forgiving and automatable.

  • Component Function
  • Power source (CV) Holds voltage; regulates arc length automatically
  • Wire feeder Drives solid wire at a set speed (sets amperage)
  • Gun / contact tip Delivers current, wire, and gas; tip transfers current
  • Gas cylinder & regulator Supplies and meters shielding gas (typ. 20–45 CFH)

The contact tip is a wear item the inspector should not overlook: a worn tip causes erratic current transfer and arc instability, and spatter buildup in the nozzle restricts gas flow and invites porosity, so nozzle and tip condition are part of routine equipment checks before production welding.

Metal Transfer Modes

The four transfer modes — set by voltage, current, and gas — are core exam material. The transition current is the threshold above which globular flips to spray; for ~0.045" steel wire in 90/10 Ar/CO₂ it is roughly 220–250 A .

Mode V / A Gas Behavior Best for

Short-circuit Low (≈16–22 V) CO₂ or 75/25 Wire dips into pool, shorts and re-arcs 50–200×/sec; coolest Thin steel, root, all positions

Globular Medium CO₂ Drops larger than wire fall by gravity; heavy spatter Carbon steel, flat/horizontal; rarely chosen on purpose

Spray High (≥24 V, above transition) ≥80% Ar Fine droplets stream axially; smooth, high deposition Thick steel, flat/horizontal, production

Pulsed-spray Pulsed peak/background ≥80% Ar Pulses above/below transition; spray quality at lower average heat All positions, medium-thick

Wire Classification and Shielding Gas

The carbon-steel wire spec is AWS A5.18 . Example ER70S-6 : E = electrode, R = rod, 70 = 70 ksi tensile, S = solid, 6 = chemistry (high Si/Mn deoxidizers, tolerates light mill scale). ER70S-3 is the cleaner-steel general-purpose wire.

  • Gas Behavior Use
  • 100% CO₂ Deep penetration, most spatter, cheap Carbon steel, short-circuit, outdoors
  • 75% Ar / 25% CO₂ (C25) Balanced penetration/spatter Most common all-around steel mix
  • 90% Ar / 10% CO₂ Low spatter, supports spray Carbon steel spray transfer
  • 100% Argon Smooth, shallow Aluminum, (with He) stainless
  • Ar/He Hotter, deeper Thick aluminum, copper

Exam trap: Pure spray transfer needs ≥80% argon — it will NOT occur in 100% CO₂. And remember CV power, not CC. A worked heat input: 250 A, 28 V, 14 ipm → (28 × 250 × 60)/14 = 30,000 J/in (30 kJ/in) .

Variants, Variables, and Inspection

GMAW has several named variants the exam may reference. 1 does not prequalify GMAW-S — it must be qualified by testing — precisely because of its incomplete-fusion tendency. Other related modes include the surface-tension-transfer and other controlled-short-circuit waveforms that modern inverters provide for root passes. Beyond gas and mode, the welder/WPS controls wire-feed speed (amperage) , voltage , contact-tip-to-work distance (CTWD/stickout) , gun travel and work angles , and gas flow rate (too low invites porosity; too high causes turbulence that pulls in air).

Common GMAW discontinuities the CWI watches for: cold lap / incomplete fusion in short-circuit mode (low heat), wormhole/whisker porosity and wire stubbing , excessive convexity in vertical-up welds, and porosity when wind, low flow, a clogged nozzle, or spatter buildup disrupts gas coverage. Because GMAW leaves no slag, surface inspection is easier than SMAW or FCAW, but incomplete fusion hidden beneath a sound-looking cap is the chronic concern — one reason production codes often require volumetric NDE (RT or UT) on critical short-circuit GMAW joints.

  • Advantages Limitations
  • High deposition; 90–95% efficiency Wind disrupts gas shielding
  • Continuous wire, little downtime More equipment than SMAW
  • Lower skill than SMAW; easily robotized Cold-lap risk in short-circuit mode