Study guide

1.6 Other Welding, Cutting Processes, and Process Variables

AWS CWI Certified Welding Inspector Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction to the AWS CWI Certification

What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application

2 1. Welding Processes and Fundamentals

1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables

3 2. Welding Metallurgy and Heat Control

2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress

4 3. Weld Discontinuities and Defects

3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile

5 4. Nondestructive Examination (NDE) Methods

4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)

6 5. Welding Symbols and Terminology

5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology

7 6. WPS, PQR, and Welder Qualification

6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)

8 7. Destructive Testing Methods

7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing

9 8. Welding Safety and Inspector Duties

8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations

10 9. AWS D1.1 Code Application (Part C)

9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation

11 10. Exam Strategies and Comprehensive Review

10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions

1.6 Other Welding, Cutting Processes, and Process Variables

Key Takeaways Explain This Topic AI

Heat Input = (Volts × Amps × 60) ÷ travel speed; e.g., 26 V × 200 A ÷ 10 ipm = 31,200 J/in (31.2 kJ/in)

Higher travel speed lowers heat input (inverse), raising HAZ cooling rate and hardness

Oxyfuel flames: neutral (steel), carburizing (excess acetylene), oxidizing (excess O₂); OFC cuts carbon steel only

Brazing/soldering are divided at 840°F (450°C) and never melt the base metal

ESW needs PWHT (high heat input); CAC-A is the inspector's tool for back-gouging and defect removal; PAC cuts all metals

Last updated: June 2026

Beyond the Five Arc Processes

The CWI exam also covers oxyfuel, brazing/soldering, resistance, electroslag, stud welding, thermal cutting, and the process variables that tie them all together.

Oxyfuel Welding and Cutting (OFW / OFC)

Oxyfuel burns a fuel gas (usually acetylene ) with oxygen to weld or cut. A neutral oxy-acetylene flame reaches about 5,600–6,300°F (≈3,100–3,480°C) . The flame setting is exam-tested:

  • Flame O₂:Fuel Use
  • Neutral ~1:1 Most steels — no chemical effect on the weld
  • Carburizing (reducing) Excess acetylene Hardfacing, high-carbon steel, some non-ferrous
  • Oxidizing Excess oxygen Brass, bronze, some copper; hottest

Oxyfuel cutting (OFC) does not melt steel — it oxidizes (burns) preheated metal and blows the iron-oxide slag out of the kerf. It works only on metals that oxidize readily , i.e., carbon and low-alloy steels. It will not cut stainless, aluminum, or copper because their oxides melt higher than the base metal (chromium oxide on stainless; Al₂O₃ at ~3,700°F vs. aluminum at ~1,220°F), so the reaction self-extinguishes. OFC requires: ignition temperature below melting point, oxide melting point below base-metal melting point, an exothermic reaction, and fluid slag.

Brazing and Soldering

Both join metal without melting the base metal , using a filler that wets the joint by capillary action. The dividing line is 840°F (450°C) : brazing uses filler that melts above 840°F ; soldering uses filler that melts below 840°F . Both rely on flux to clean oxides and proper joint clearance (typ. 006") for capillary flow. Because the base metal never melts, brazed and soldered joints are inspected differently from fusion welds — the inspector looks for full capillary fill, wetting, and the absence of voids rather than fusion-line indications.

Common brazing fillers include silver (BAg), copper-phosphorus (BCuP, self-fluxing on copper), and brass (RBCuZn); common solders are tin-based alloys. A frequent exam distinction: braze welding deposits filler into a groove or fillet like fusion welding (no capillary action) yet still keeps the base metal below its melting point — it is not the same as capillary brazing.

Other Processes and Thermal Cutting

  • Process Principle Application
  • RSW (resistance spot) Current + pressure through overlap; resistance heat Auto body, sheet metal
  • RSEW (resistance seam) Rotating wheel electrodes, continuous seam Tanks, cans
  • FW (flash welding) Flash, then forge under upset Rails, chain, band-saw blades

ESW (electroslag) Molten slag carries current, vertical-up, copper shoes Thick plate (1"–12"+) in one pass; very high heat input → PWHT usually required

  • SW (stud welding) Drawn-arc or capacitor discharge Shear connectors (AWS D1.1 Clause 9)
  • PAC (plasma arc cut) Constricted ionized gas jet All metals incl. stainless, aluminum

CAC-A (air carbon arc) Carbon electrode melts metal; 80–100 psi air blows it out Back-gouging, defect removal, repair prep

ESW and CAC-A matter most to inspectors: ESW's extreme heat input drives grain growth and usually mandates PWHT; CAC-A is the primary method for back-gouging a groove root and for removing defective welds before repair. One CAC-A caution the CWI enforces: gouging leaves a carbon-enriched, hardened layer on the cut surface, so the groove must be ground clean before rewelding to avoid carbon pickup and cracking.

Choosing a Process — Comparative Summary

The inspector is often asked why a given process was specified. The quick mental map below ties the chapter together:

  • Need Typical choice
  • Field repair, portability SMAW
  • High-deposition shop fabrication GMAW (spray) or FCAW-G
  • Windy outdoor erection FCAW-S or SMAW
  • Highest weld quality, thin/exotic metal GTAW
  • Long straight high-volume seams (flat) SAW
  • Thick plate in a single vertical pass ESW

Each choice trades deposition rate, position capability, portability, and quality against one another — exactly the factors a WPS balances.

Process Variables and Heat Input

The three master arc variables are current (amperage) , arc voltage , and travel speed :

Current drives penetration and deposition — raise it for deeper, hotter welds.

Voltage controls arc length and bead width — higher voltage widens and flattens the bead.

Travel speed is inversely related to heat — faster travel = less heat per inch, narrower bead, but too fast causes undercut/incomplete fusion.

These combine in the heat input formula that WPSs and codes (e.g., AWS D1.1) limit to control HAZ properties:

Heat Input (J/in) = (Volts × Amps × 60) ÷ Travel Speed (in/min)

The 60 converts seconds to minutes so the answer comes out in joules per inch (divide by 1,000 for kJ/in). Worked example: a weld run at 26 V , 200 A , traveling 10 ipm :

Heat Input = (26 × 200 × 60) ÷ 10 = 312,000 ÷ 10 = 31,200 J/in = 31.2 kJ/in

If travel speed doubles to 20 ipm at the same volts and amps, heat input halves to 15.6 kJ/in — faster travel cools the joint, raising the cooling rate and hardness in the HAZ. This inverse relationship is a favorite Part A calculation.

Exam trap: OFC cuts carbon steel only , not stainless/aluminum/copper; PAC cuts all metals; CAC-A is for back-gouging and defect removal; the brazing/soldering line is 840°F .