Study guide
1.5 SAW — Submerged Arc Welding
AWS CWI Certified Welding Inspector Exam
Track your progress as you read
Finished sections get a check mark.
1 Introduction to the AWS CWI Certification
What Is the AWS CWI Certification? CWI Exam Structure: Parts A, B, and C Eligibility Requirements and Application
2 1. Welding Processes and Fundamentals
1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables
3 2. Welding Metallurgy and Heat Control
2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress
4 3. Weld Discontinuities and Defects
3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile
5 4. Nondestructive Examination (NDE) Methods
4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)
6 5. Welding Symbols and Terminology
5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology
7 6. WPS, PQR, and Welder Qualification
6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)
8 7. Destructive Testing Methods
7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing
9 8. Welding Safety and Inspector Duties
8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations
10 9. AWS D1.1 Code Application (Part C)
9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation
11 10. Exam Strategies and Comprehensive Review
10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions
1.5 SAW — Submerged Arc Welding
Key Takeaways Explain This Topic AI
SAW buries the arc under granular flux — no visible arc, spatter, or UV — on a CV (or CC) source
Highest single-arc deposition rate: 25–100+ lbs/hr, but flat and horizontal positions only
AWS A5.17 classifies wire+flux together (e.g., F7A2-EL12: 70 ksi, as-welded, 20 ft-lb at −20°F)
Three flux types: fused (non-hygroscopic), bonded and agglomerated (can alloy but absorb moisture)
- High heat input demands HAZ/cooling-rate control; bonded fluxes held heated to prevent hydrogen cracking
- Last updated: September 2026
Submerged Arc Welding (SAW)
Submerged Arc Welding (SAW) is the high-production, mechanized process in which the arc burns entirely beneath a blanket of granular flux — hence "submerged." Because the flux hides the arc, there is no visible arc, no spatter, and no ultraviolet radiation , and the process posts the highest deposition rate of any single-arc process, 25–100+ lbs/hr . It is the backbone of plate girders, pressure-vessel shells, pipe seams, and wind-tower fabrication.
A bare solid or metal-cored wire is fed continuously into the joint while a hopper lays granular flux ahead of and around it. The arc melts wire, base metal, and part of the flux into a pool; the molten flux becomes a glassy slag and the unmelted flux is vacuumed up and recycled. Most SAW runs on constant voltage (CV) for smaller wires (self-regulating, like GMAW), while large-diameter wire often uses constant current (CC) with voltage-sensing feed.
A practical consequence of burying the arc is that operator fume and arc-flash exposure are very low , but it also means the weld must be set up so precisely on the joint line that even a small mistracking can run the bead off the seam unseen.
SAW is highly adaptable to multi-electrode arrangements that push deposition even higher. Tandem SAW runs two or more wires in line — typically the lead wire on DC for penetration and a trail wire on AC for fill and bead shape — and twin/parallel setups feed two wires through one contact tip. Cold-wire and hot-wire additions and iron-powder fill can further raise deposition without adding arc energy. The inspector should appreciate that these productivity boosts also raise total heat input and the risk of inter-run slag entrapment, so parameter control and inter-pass cleaning are scrutinized.
- Component Function
- Power source (CV or CC) Supplies the high currents SAW needs
- Wire feeder Drives electrode from coils or drums
- Flux hopper Deposits granular flux to bury the arc
- Flux recovery Vacuums and recycles unfused flux
- Travel carriage Tractor, side-beam, or gantry for mechanized travel
Because SAW is mechanized, the operator's role shifts from manual bead control to setup, parameter monitoring, and joint tracking , which is why operator-qualification and machine-calibration records become central to the inspector's documentation review.
Operating Parameters
- Parameter Typical Effect
- Current 300–2,000+ A Penetration and deposition
- Voltage 28–40 V Bead width, flux consumption
- Travel speed 10–120+ ipm Bead width, penetration, heat input
- Wire diameter 3/32"–1/4" Current capacity
- Stickout (CTWD) ~1"–1.5" Resistive preheat, deposition
Consumables, Flux Types, and Limits
SAW wire/flux are classified together under AWS A5.17 (carbon steel). The wire EL12 means E lectrode, L low manganese, 12 = ~0.12% carbon. The flux-wire combination is what gets certified for mechanical properties.
Flux-wire example: F7A2-EL12
- Character Meaning
- F Flux
- 7 70 ksi minimum tensile
- A As-welded (P = after PWHT)
- 2 Charpy ≥ 20 ft-lb at −20°F
- EL12 Electrode classification
- Flux type How made Behavior
- Fused Melted, then crushed Homogeneous, non-hygroscopic, recycles well; cannot add deoxidizers
- Bonded Bonded with binder, baked Can add deoxidizers/alloys; hygroscopic (absorbs moisture)
- Agglomerated Similar to bonded Can add alloys; moderate moisture pickup
- Positions and Inspection
SAW's defining limitation: it is flat (1G/1F) and horizontal (2F) only , because the loose granular flux must rest on the joint by gravity — it cannot be made to stay on a vertical or overhead surface. It also suits only long, straight, or circular (rotated) seams, and on circumferential pipe seams the workpiece is rotated under a fixed head so the weld stays at top dead center. Thick SAW joints are frequently welded from both sides, which makes back-gouging of the first side (usually by CAC-A) before the second pass a routine step the CWI verifies for complete joint penetration.
Because the arc is hidden, the operator cannot watch the puddle, so mechanical tracking, controlled parameters, and downstream NDE carry the quality burden. Inspectors watch for slag inclusions between SAW passes (multi-wire/tandem setups are common), lack of fusion at high travel speeds, and hydrogen cracking if bonded/agglomerated flux has picked up moisture — which is why such flux is held in heated hoppers. Heat input must also be controlled : arc energy per unit length depends on voltage, current, and travel speed. For steady conditions, arc energy in kJ/in is 60VI/(1000v), with v in in/min. Apply any process-efficiency factor required by the specified method, and compare the result with the WPS limits; do not assume one heat-input value fits every SAW weld.
Exam trap: SAW is flat and horizontal only (gravity holds the flux). It has the highest single-arc deposition rate but cannot weld vertical or overhead.
- Advantages Limitations
- Highest deposition (25–100+ lbs/hr) Flat/horizontal only
- No visible arc, spatter, or UV Straight/circular seams only
- Deep penetration (to ~1" single pass) Cannot watch the puddle
- Excellent, consistent bead Flux moisture/handling complexity
A5.17 Flux-Wire Classification and Flux Manufacture
The flux is half of the SAW consumable system, and how it is made governs both what it can do metallurgically and how it must be handled. The three manufacturing routes give very different behavior:
Flux type How made Can add alloys? Moisture pickup Notes
Fused Ingredients melted together, then crushed and screened No (melting destroys deoxidizers) Very low (non-hygroscopic) Recycles well, consistent, but cannot deoxidize the pool
Bonded Dry ingredients bound with silicate, baked at low temperature Yes — deoxidizers and alloys survive Higher (hygroscopic) Lower density; must be kept dry, heated hoppers
Agglomerated Pelletized with a binder, similar to bonded Yes Moderate European term largely overlapping "bonded"
Because bonded and agglomerated fluxes can carry deoxidizers and alloying additions, they let a fabricator tune weld-metal chemistry — but they also absorb moisture , which is a direct hydrogen-cracking risk, so they are stored sealed and run from heated hoppers . Fused flux trades that flexibility for stability.
Decoding F7A2-EL12
The full SAW flux-wire designation pairs a flux property string with the electrode. F7A2-EL12 reads as: F = flux; 7 = 70 ksi minimum tensile (and a defined yield/elongation set); A = tested in the as-welded condition (a P here would mean tested after PWHT); 2 = Charpy V-notch of at least 20 ft-lb at −20°F ; EL12 = a low-manganese ( L ) solid electrode of about 0.12% carbon . The same flux can earn different ratings with different wires, which is why the flux-wire combination , not the wire alone, is what gets certified for mechanical properties.
Multi-Wire and Tandem Productivity
SAW scales deposition far beyond a single arc. Tandem SAW runs the lead wire on DC for penetration and a trailing wire on AC for fill and bead shape; twin/parallel setups feed two wires through one tip; cold- and hot-wire additions and iron-powder fill raise deposition without raising arc energy. These arrangements drive deposition into the 25–100+ lb/hr range and let single-pass penetration reach roughly 1 inch, but they also raise total heat input and the chance of inter-run slag entrapment, so the inspector scrutinizes parameter control and interpass cleaning.
The Flat/Horizontal Limitation
SAW's defining restriction follows directly from physics: the loose granular flux is held in the joint only by gravity , so the process is limited to flat (1G/1F) and, with care, horizontal (2F) positions and cannot be made to weld vertical or overhead. It therefore suits long straight seams and circular seams welded with the work rotated under a fixed head so the puddle stays at top dead center.