2 1. Welding Processes and Fundamentals

1.1 SMAW — Shielded Metal Arc Welding (Stick) 1.2 GMAW — Gas Metal Arc Welding (MIG/MAG) 1.3 FCAW — Flux-Cored Arc Welding 1.4 GTAW — Gas Tungsten Arc Welding (TIG) 1.5 SAW — Submerged Arc Welding 1.6 Other Welding, Cutting Processes, and Process Variables

3 2. Welding Metallurgy and Heat Control

2.1 The Iron-Carbon Phase Diagram 2.2 The Heat-Affected Zone (HAZ) 2.3 Preheat and Interpass Temperature 2.4 Hydrogen-Induced Cracking (HIC) 2.5 Distortion and Residual Stress

4 3. Weld Discontinuities and Defects

3.1 Discontinuity vs. Defect — Definitions and Concepts 3.2 Cracks — Types, Causes, and Significance 3.3 Porosity and Inclusions 3.4 Incomplete Fusion and Incomplete Joint Penetration 3.5 Geometric Discontinuities: Undercut, Overlap, and Profile

5 4. Nondestructive Examination (NDE) Methods

4.1 Visual Testing (VT) 4.2 Liquid Penetrant Testing (PT) 4.3 Magnetic Particle Testing (MT) 4.4 Radiographic Testing (RT) and Ultrasonic Testing (UT)

6 5. Welding Symbols and Terminology

5.1 Anatomy of a Welding Symbol (AWS A2.4) 5.2 Joint Types, Weld Types, and Welding Positions 5.3 Essential Welding Definitions and Terminology

7 6. WPS, PQR, and Welder Qualification

6.1 Welding Procedure Specification (WPS) 6.2 Procedure Qualification Record (PQR) 6.3 Welder Performance Qualification (WPQ)

8 7. Destructive Testing Methods

7.1 Tensile Testing 7.2 Guided Bend, Nick Break, and Fillet Weld Break Tests 7.3 Impact Testing and Hardness Testing

9 8. Welding Safety and Inspector Duties

8.1 Welding Safety Hazards and Prevention 8.2 CWI Duties and Responsibilities 8.3 Welding-Related Calculations

10 9. AWS D1.1 Code Application (Part C)

9.1 AWS D1.1:2025 Code Structure and Navigation 9.2 Clause 5 — Prequalification Requirements 9.3 Clause 8 — Inspection and Acceptance Criteria 9.4 Part B Practical Exam Preparation

11 10. Exam Strategies and Comprehensive Review

10.1 Part A (Fundamentals) Exam Strategies 10.2 Part C (Code Application) Exam Strategies 10.3 Comprehensive Review — 25 Practice Questions

6.3 Welder Performance Qualification (WPQ)

Key Takeaways Explain This Topic AI

A WPQ qualifies the welder's SKILL; a PQR qualifies the PROCEDURE — both are required before production

WPQ uses bend, radiography, macro-etch, or fillet-break tests (always VT first) — never tensile tests

Position follows 'harder qualifies easier': 6G pipe, or 3G + 4G plate, qualifies ALL positions (Table 6.10)

A 1 in (25 mm) test plate qualifies unlimited production thickness (Table 6.11), like the PQR rule

Clause 6.4.1: qualification lapses after 6 months of process inactivity, but one retest restores all positions; the CWI verifies each WPQ covers the production process, position, thickness, and filler

Last updated: June 2026

What a WPQ Is

A Welder Performance Qualification (WPQ) — also called a welder qualification test record — verifies that an individual welder has the skill to deposit sound weld metal following a WPS. This is a fundamental distinction the CWI exam hammers: a PQR qualifies the procedure , while a WPQ qualifies the person . Both must exist before production: the procedure must be proven capable, and each welder must be proven able to execute it.

The welder makes a test coupon under a qualified WPS; the coupon is then evaluated. Because the goal is to judge soundness of deposit (not the joint's strength — that was already proven by the PQR), the WPQ relies on bend tests, radiography, macro-etch, or fillet break tests , not tensile tests.

  • Feature PQR (Procedure) WPQ (Welder)
  • What is qualified The welding procedure/variables The individual welder's skill
  • Typical tests Tensile + bend (+ CVN if specified) Bend or RT; macro/break for fillets; always VT first
  • Scope One per procedure One per welder, per process, per position group
  • Lapses? No — only on essential change Yes — by inactivity (6-month rule) or quality concern
  • WPQ Test Methods
  • Method When Used
  • Visual (VT) Always first — gross defects fail the coupon before destructive testing
  • Guided bend Standard for groove qualification (root/face, or side bends for thicker plate)
  • Radiography (RT) Permitted in lieu of bends for groove coupons under D1.1
  • Macro-etch Fillet weld qualification — checks fusion and profile on a cut cross-section
  • Fillet break test Fillet coupon is fractured and the exposed surface examined for soundness
  • Position Qualification Ranges (Table 6.10)

Welding position is an essential variable for the welder, and the code follows a "harder qualifies easier" logic. Vertical (3G) and overhead (4G) are the difficult positions, so qualifying in them extends to flat and horizontal.

  • Test Position(s) Production Positions Qualified
  • 1G (flat plate) Flat groove only
  • 2G Flat + horizontal
  • 3G + 4G (plate) All positions (flat, horizontal, vertical, overhead)
  • 6G (pipe, 45° fixed) All positions — the most versatile single test

A welder who passes a 6G pipe test, or a 3G plus 4G plate combination, is qualified for all groove and fillet positions — the most exam-cited fact in this topic.

Thickness Qualification (Table 6.11)

  • Test Plate Thickness (T) Production Thickness Qualified
  • 1/8 in (3 mm) ≤ T < 1 in (25 mm) 1/8 in (3 mm) min to 2T max
  • T ≥ 1 in (25 mm) 1/8 in (3 mm) min to unlimited

A welder tested on a 1 in plate is therefore qualified for unlimited thickness — mirroring the PQR rule and frequently tested side by side with it.

Essential Variables for the Welder

  • Essential Variable Change Requiring Requalification
  • Process SMAW → GMAW, or any process switch
  • Position Adding a position not covered (per Table 6.10 logic)
  • Filler F-number Moving to a higher/different F-number group
  • Vertical progression Uphill ↔ downhill
  • Backing Removing backing (welding without it) when qualified with it
  • Thickness Production thickness outside the qualified range
  • Maintaining Qualification — The 6-Month Rule

Per AWS D1.1 Clause 6.4.1 , a welder's qualification stays valid as long as: (1) the welder has used that process within the previous 6 months ; (2) there is no specific reason to question the welder's ability (e.g., repeated rejects); and (3) the essential variables have not changed beyond range. If the 6-month activity lapses, qualification expires for that process — but a single requalification coupon (e.g., on a 1 in plate) can restore all positions .

Diameter, Backing, and Record Contents

For pipe and tube , qualification also depends on outside diameter, and the CWI checks the diameter range as carefully as the thickness range. The backing condition matters too: a welder qualified with backing is not automatically qualified to weld without backing (an open-root joint), because the open-root root pass is a distinct, harder skill — a frequent exam distractor. A complete WPQ record documents the welder's stamp, the WPS followed, the actual process/position welded, base and filler metals, coupon thickness/diameter, test method and results, the qualified ranges, and the witnessing signatory.

Like the PQR it is a historical record , but unlike the PQR it has a shelf life governed by the 6-month activity rule.

The CWI's Role

The CWI's job in performance qualification is verification, not training or welding . Before and during production the inspector confirms each welder's WPQ record is current and covers the process, position, thickness range, diameter, filler F-number, and backing condition of the actual production joint. A welder qualified only on 3G plate cannot be assigned overhead production without 4G coverage; a welder qualified only with backing cannot be put on open-root work; a CWI who allows either has failed the core duty.

The inspector also confirms the welder's continuity (that the 6-month rule has not lapsed) and that no quality concern has invalidated the qualification.

Exam trap: Do not confuse the documents — PQR qualifies the procedure; WPQ qualifies the welder. And remember the qualification restores after a lapse with one retest; lapsing does not erase the welder's history, only the current validity.